Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Density | 20 °C | 7.84 g/cm³ Show Material materials with Density of 7.84 g/cm³ | normalized or normalized formed (+N) | EN 10028-3 | Sheet, Flat |
Mechanical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elastic modulus | -100 °C | 217 GPa Show Material materials with Elastic modulus of 217 GPa | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | |
20 °C | 210 GPa Show Material materials with Elastic modulus of 210 GPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 210 - 212 GPa Show Material materials with Elastic modulus of 210 - 212 GPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 212 GPa Show Material materials with Elastic modulus of 212 GPa | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | ||
100 °C | 207 GPa Show Material materials with Elastic modulus of 207 GPa | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | ||
200 °C | 199 GPa Show Material materials with Elastic modulus of 199 GPa | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | ||
300 °C | 192 GPa Show Material materials with Elastic modulus of 192 GPa | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | ||
400 °C | 184 GPa Show Material materials with Elastic modulus of 184 GPa | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | ||
500 °C | 175 GPa Show Material materials with Elastic modulus of 175 GPa | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | ||
600 °C | 164 GPa Show Material materials with Elastic modulus of 164 GPa | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | ||
Elongation | 13.9 % Show Material materials with Elongation of 13.9 % | Predicted Value, A200 | ||||
15.4 % Show Material materials with Elongation of 15.4 % | Predicted Value, A80 | |||||
16.4 % Show Material materials with Elongation of 16.4 % | Predicted Value, A80 Transverse | |||||
20.0 % Show Material materials with Elongation of 20.0 % | Predicted Value, A50 | |||||
20.9 % Show Material materials with Elongation of 20.9 % | Predicted Value, A5 | |||||
20 °C | 16 % Show Material materials with Elongation of 16 % | normalized or normalized formed (+N) | EN 10028-3 | Sheet, Flat | ||
20 °C | 17 % Show Material materials with Elongation of 17 % | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 17 % Show Material materials with Elongation of 17 % | normalized or normalized formed (+N) | EN 10028-3 | Sheet | Transverse | |
Hardness, Brinell | 252 [-] Show Material materials with Hardness, Brinell of 252 [-] | Predicted Value, Transverse | ||||
Poisson's ratio | 0.3 [-] Show Material materials with Poisson's ratio of 0.3 [-] | Typical for Steel | ||||
Reduction of area | 38.7 % Show Material materials with Reduction of area of 38.7 % | Predicted Value | ||||
44.0 % Show Material materials with Reduction of area of 44.0 % | Predicted Value, Transverse | |||||
Shear modulus | 80.3 GPa Show Material materials with Shear modulus of 80.3 GPa | Predicted Value | ||||
Shear strength | 547.9 MPa Show Material materials with Shear strength of 547.9 MPa | Predicted Value | ||||
Tensile strength | 20 °C | 510 - 690 MPa Show Material materials with Tensile strength of 510 - 690 MPa | normalized or normalized formed (+N) | EN 10028-3 | Sheet, Flat | |
20 °C | 510 - 720 MPa Show Material materials with Tensile strength of 510 - 720 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 510 - 710 MPa Show Material materials with Tensile strength of 510 - 710 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 520 - 720 MPa Show Material materials with Tensile strength of 520 - 720 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 520 - 710 MPa Show Material materials with Tensile strength of 520 - 710 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 520 - 690 MPa Show Material materials with Tensile strength of 520 - 690 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 540 - 720 MPa Show Material materials with Tensile strength of 540 - 720 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 540 - 710 MPa Show Material materials with Tensile strength of 540 - 710 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 540 - 690 MPa Show Material materials with Tensile strength of 540 - 690 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 570 - 720 MPa Show Material materials with Tensile strength of 570 - 720 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 570 - 710 MPa Show Material materials with Tensile strength of 570 - 710 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 570 - 690 MPa Show Material materials with Tensile strength of 570 - 690 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 630 - 725 MPa Show Material materials with Tensile strength of 630 - 725 MPa | normalized or normalized formed (+N) | EN 10028-3 | Sheet | Transverse | |
Yield strength | 283.5 MPa Show Material materials with Yield strength of 283.5 MPa | Predicted Value, RP1 | ||||
315.1 MPa Show Material materials with Yield strength of 315.1 MPa | Predicted Value, RP1 Transverse | |||||
432 MPa Show Material materials with Yield strength of 432 MPa | Predicted Value, RP02 | |||||
465.3 MPa Show Material materials with Yield strength of 465.3 MPa | Predicted Value, RP02 Transverse | |||||
507.1 MPa Show Material materials with Yield strength of 507.1 MPa | Predicted Value, RP002 | |||||
520.9 MPa Show Material materials with Yield strength of 520.9 MPa | Predicted Value, RP05 | |||||
20 °C | 370 MPa Show Material materials with Yield strength of 370 MPa | normalized or normalized formed (+N) | EN 10028-3 | Sheet, Flat | ||
20 °C | 380 MPa Show Material materials with Yield strength of 380 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 400 MPa Show Material materials with Yield strength of 400 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 430 MPa Show Material materials with Yield strength of 430 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 445 MPa Show Material materials with Yield strength of 445 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 460 MPa Show Material materials with Yield strength of 460 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 460 MPa Show Material materials with Yield strength of 460 MPa | normalized or normalized formed (+N) | EN 10028-3 | Sheet | Transverse |
Thermal
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Coefficient of thermal expansion | -100 °C | 1.05e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.05e-05 1/K | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
20 °C | 1.15e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.15e-05 1/K | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | |
100 °C | 1.21e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.21e-05 1/K | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | |
200 °C | 1.27e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.27e-05 1/K | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | |
300 °C | 1.32e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.32e-05 1/K | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | |
400 °C | 1.36e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.36e-05 1/K | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | |
500 °C | 1.4e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.4e-05 1/K | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | |
600 °C | 1.44e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.44e-05 1/K | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | |
Specific heat capacity | -100 °C | 423 J/(kg·K) Show Material materials with Specific heat capacity of 423 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
20 °C | 430 J/(kg·K) Show Material materials with Specific heat capacity of 430 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
20 °C | 430 - 461 J/(kg·K) Show Material materials with Specific heat capacity of 430 - 461 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
20 °C | 461 J/(kg·K) Show Material materials with Specific heat capacity of 461 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | |
100 °C | 479 J/(kg·K) Show Material materials with Specific heat capacity of 479 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | |
200 °C | 499 J/(kg·K) Show Material materials with Specific heat capacity of 499 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | |
300 °C | 517 J/(kg·K) Show Material materials with Specific heat capacity of 517 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | |
400 °C | 536 J/(kg·K) Show Material materials with Specific heat capacity of 536 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | |
500 °C | 558 J/(kg·K) Show Material materials with Specific heat capacity of 558 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | |
600 °C | 587 J/(kg·K) Show Material materials with Specific heat capacity of 587 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | |
Thermal conductivity | -100 °C | 34.7 W/(m·K) Show Material materials with Thermal conductivity of 34.7 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
20 °C | 39.7 - 40 W/(m·K) Show Material materials with Thermal conductivity of 39.7 - 40 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
20 °C | 39.7 W/(m·K) Show Material materials with Thermal conductivity of 39.7 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | |
20 °C | 40 W/(m·K) Show Material materials with Thermal conductivity of 40 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
100 °C | 40.9 W/(m·K) Show Material materials with Thermal conductivity of 40.9 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | |
200 °C | 41 W/(m·K) Show Material materials with Thermal conductivity of 41 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | |
300 °C | 39.9 W/(m·K) Show Material materials with Thermal conductivity of 39.9 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | |
400 °C | 38.2 W/(m·K) Show Material materials with Thermal conductivity of 38.2 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | |
500 °C | 36.1 W/(m·K) Show Material materials with Thermal conductivity of 36.1 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | |
600 °C | 33.8 W/(m·K) Show Material materials with Thermal conductivity of 33.8 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | |
Thermal diffusivity | -100 °C | 11.9 mm²/s Show Material materials with Thermal diffusivity of 11.9 mm²/s | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
20 °C | 11 mm²/s Show Material materials with Thermal diffusivity of 11 mm²/s | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | |
100 °C | 10.5 mm²/s Show Material materials with Thermal diffusivity of 10.5 mm²/s | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | |
200 °C | 9.9 mm²/s Show Material materials with Thermal diffusivity of 9.9 mm²/s | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | |
300 °C | 9.1 mm²/s Show Material materials with Thermal diffusivity of 9.1 mm²/s | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | |
400 °C | 8.1 mm²/s Show Material materials with Thermal diffusivity of 8.1 mm²/s | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | |
500 °C | 6.9 mm²/s Show Material materials with Thermal diffusivity of 6.9 mm²/s | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | |
600 °C | 5.7 mm²/s Show Material materials with Thermal diffusivity of 5.7 mm²/s | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Electrical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Electrical conductivity | 5 S/m Show Material materials with Electrical conductivity of 5 S/m | Predicted Value | ||||
Electrical resistivity | -100 °C | 1.97e-07 Ω·m Show Material materials with Electrical resistivity of 1.97e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | |
20 °C | 2.6e-07 Ω·m Show Material materials with Electrical resistivity of 2.6e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 2.6e-07 - 2.62e-07 Ω·m Show Material materials with Electrical resistivity of 2.6e-07 - 2.62e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 2.62e-07 Ω·m Show Material materials with Electrical resistivity of 2.62e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | ||
100 °C | 3.13e-07 Ω·m Show Material materials with Electrical resistivity of 3.13e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | ||
200 °C | 3.85e-07 Ω·m Show Material materials with Electrical resistivity of 3.85e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | ||
300 °C | 4.7e-07 Ω·m Show Material materials with Electrical resistivity of 4.7e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | ||
400 °C | 5.69e-07 Ω·m Show Material materials with Electrical resistivity of 5.69e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | ||
500 °C | 6.85e-07 Ω·m Show Material materials with Electrical resistivity of 6.85e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | ||
600 °C | 8.2e-07 Ω·m Show Material materials with Electrical resistivity of 8.2e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | 0.005 % Show Material materials with Aluminium of 0.005 % | normalized or normalized formed (+N) | EN 10028-3 | Sheet |
0.02 % Show Material materials with Aluminium of 0.02 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | |
Carbon | 0.2 % Show Material materials with Carbon of 0.2 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Chromium | 0.3 % Show Material materials with Chromium of 0.3 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Copper | 0.2 % Show Material materials with Copper of 0.2 % | normalized or normalized formed (+N) | EN 10028-3 | Sheet |
0.7 % Show Material materials with Copper of 0.7 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | |
Manganese | 1 - 1.7 % Show Material materials with Manganese of 1 - 1.7 % | normalized or normalized formed (+N) | EN 10028-3 | Sheet |
1.1 - 1.7 % Show Material materials with Manganese of 1.1 - 1.7 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | |
Molybdenum | 0.1 % Show Material materials with Molybdenum of 0.1 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Nickel | 0.4 % Show Material materials with Nickel of 0.4 % | normalized or normalized formed (+N) | EN 10028-3 | Sheet |
0.8 % Show Material materials with Nickel of 0.8 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | |
Niobium | 0.05 % Show Material materials with Niobium of 0.05 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Nitrogen | 0.025 % Show Material materials with Nitrogen of 0.025 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Phosphorus | 0.02 % Show Material materials with Phosphorus of 0.02 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
0.03 % Show Material materials with Phosphorus of 0.03 % | normalized or normalized formed (+N) | EN 10028-3 | Sheet | |
Silicon | 0.1 - 0.6 % Show Material materials with Silicon of 0.1 - 0.6 % | normalized or normalized formed (+N) | EN 10028-3 | Sheet |
0.6 % Show Material materials with Silicon of 0.6 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | |
Sulfur | 0.01 % Show Material materials with Sulfur of 0.01 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
0.02 % Show Material materials with Sulfur of 0.02 % | normalized or normalized formed (+N) | EN 10028-3 | Sheet | |
Titanium | 0.03 % Show Material materials with Titanium of 0.03 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Vanadium | 0.1 - 0.2 % Show Material materials with Vanadium of 0.1 - 0.2 % | normalized or normalized formed (+N) | EN 10028-3 | Sheet |
0.2 % Show Material materials with Vanadium of 0.2 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Technological properties
Property | ||
---|---|---|
Supplier Disclaimer | The given information is a rough description and some properties can depend on various factors such as product thickness. Please contact the supplier or refer to the related norm or standard for further information. |
Do you have a technical question or need more information about this material?
Post it as a comment below and receive answers from engineers and other community members.