General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Density | 20 °C | 7.85 g/cm³ Show Material materials with Density of 7.85 g/cm³ | normalized and tempered (+NT) | EN 10028-4 | Flat |
Mechanical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elastic modulus | -100 °C | 217 GPa Show Material materials with Elastic modulus of 217 GPa | normalized and tempered (+NT) | EN 10028-4 | Flat | |
20 °C | 212 GPa Show Material materials with Elastic modulus of 212 GPa | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
100 °C | 207 GPa Show Material materials with Elastic modulus of 207 GPa | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
200 °C | 199 GPa Show Material materials with Elastic modulus of 199 GPa | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
300 °C | 192 GPa Show Material materials with Elastic modulus of 192 GPa | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
400 °C | 184 GPa Show Material materials with Elastic modulus of 184 GPa | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
500 °C | 175 GPa Show Material materials with Elastic modulus of 175 GPa | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
600 °C | 164 GPa Show Material materials with Elastic modulus of 164 GPa | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
Elongation | 17.3 % Show Material materials with Elongation of 17.3 % | Predicted Value, A80 | ||||
17.3 % Show Material materials with Elongation of 17.3 % | Predicted Value, A80 Transverse | |||||
18.0 % Show Material materials with Elongation of 18.0 % | Predicted Value, A200 | |||||
20.1 % Show Material materials with Elongation of 20.1 % | Predicted Value, Transverse | |||||
20.3 % Show Material materials with Elongation of 20.3 % | Predicted Value, A50 | |||||
21.1 % Show Material materials with Elongation of 21.1 % | Predicted Value, A5 | |||||
20 °C | 22 % Show Material materials with Elongation of 22 % | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
Poisson's ratio | 0.291 [-] Show Material materials with Poisson's ratio of 0.291 [-] | Typical for Nickel Steel | ||||
Reduction of area | 39.6 % Show Material materials with Reduction of area of 39.6 % | Predicted Value | ||||
44.2 % Show Material materials with Reduction of area of 44.2 % | Predicted Value, Transverse | |||||
Shear modulus | 76 GPa Show Material materials with Shear modulus of 76 GPa | Typical for Nickel Steel | ||||
Shear strength | 532.4 MPa Show Material materials with Shear strength of 532.4 MPa | Predicted Value | ||||
Tensile strength | 20 °C | 490 - 610 MPa Show Material materials with Tensile strength of 490 - 610 MPa | normalized and tempered (+NT) | EN 10028-4 | Flat | |
Yield strength | 257.8 MPa Show Material materials with Yield strength of 257.8 MPa | Predicted Value, RP1 | ||||
300.3 MPa Show Material materials with Yield strength of 300.3 MPa | Predicted Value, RP1 Transverse | |||||
366.3 MPa Show Material materials with Yield strength of 366.3 MPa | Predicted Value, Transverse | |||||
369.8 MPa Show Material materials with Yield strength of 369.8 MPa | Predicted Value, RP02 | |||||
423.7 MPa Show Material materials with Yield strength of 423.7 MPa | Predicted Value, RP05 | |||||
464.5 MPa Show Material materials with Yield strength of 464.5 MPa | Predicted Value, RP002 | |||||
466.6 MPa Show Material materials with Yield strength of 466.6 MPa | Predicted Value, RP02 Transverse | |||||
20 °C | 335 MPa Show Material materials with Yield strength of 335 MPa | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
20 °C | 345 MPa Show Material materials with Yield strength of 345 MPa | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
20 °C | 355 MPa Show Material materials with Yield strength of 355 MPa | normalized and tempered (+NT) | EN 10028-4 | Flat |
Thermal
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coefficient of thermal expansion | -100 °C | 1.05e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.05e-05 1/K | normalized and tempered (+NT) | EN 10028-4 | Flat | |
20 °C | 1.15e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.15e-05 1/K | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
100 °C | 1.21e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.21e-05 1/K | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
200 °C | 1.27e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.27e-05 1/K | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
300 °C | 1.32e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.32e-05 1/K | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
400 °C | 1.36e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.36e-05 1/K | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
500 °C | 1.4e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.4e-05 1/K | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
600 °C | 1.44e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.44e-05 1/K | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
Melting point | 1316 - 1595 °C Show Material materials with Melting point of 1316 - 1595 °C | Typical for Nickel Steel | ||||
Specific heat capacity | -100 °C | 423 J/(kg·K) Show Material materials with Specific heat capacity of 423 J/(kg·K) | normalized and tempered (+NT) | EN 10028-4 | Flat | |
20 °C | 461 J/(kg·K) Show Material materials with Specific heat capacity of 461 J/(kg·K) | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
100 °C | 479 J/(kg·K) Show Material materials with Specific heat capacity of 479 J/(kg·K) | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
200 °C | 499 J/(kg·K) Show Material materials with Specific heat capacity of 499 J/(kg·K) | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
300 °C | 517 J/(kg·K) Show Material materials with Specific heat capacity of 517 J/(kg·K) | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
400 °C | 536 J/(kg·K) Show Material materials with Specific heat capacity of 536 J/(kg·K) | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
500 °C | 558 J/(kg·K) Show Material materials with Specific heat capacity of 558 J/(kg·K) | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
600 °C | 587 J/(kg·K) Show Material materials with Specific heat capacity of 587 J/(kg·K) | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
Thermal conductivity | 20 °C | 42.5 W/(m·K) Show Material materials with Thermal conductivity of 42.5 W/(m·K) | normalized and tempered (+NT) | EN 10028-4 | Flat | |
100 °C | 43.5 W/(m·K) Show Material materials with Thermal conductivity of 43.5 W/(m·K) | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
200 °C | 42.8 W/(m·K) Show Material materials with Thermal conductivity of 42.8 W/(m·K) | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
300 °C | 40.9 W/(m·K) Show Material materials with Thermal conductivity of 40.9 W/(m·K) | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
400 °C | 39 W/(m·K) Show Material materials with Thermal conductivity of 39 W/(m·K) | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
500 °C | 36.4 W/(m·K) Show Material materials with Thermal conductivity of 36.4 W/(m·K) | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
600 °C | 34.1 W/(m·K) Show Material materials with Thermal conductivity of 34.1 W/(m·K) | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
Thermal diffusivity | 20 °C | 11.7 mm²/s Show Material materials with Thermal diffusivity of 11.7 mm²/s | normalized and tempered (+NT) | EN 10028-4 | Flat | |
100 °C | 11.2 mm²/s Show Material materials with Thermal diffusivity of 11.2 mm²/s | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
200 °C | 10.3 mm²/s Show Material materials with Thermal diffusivity of 10.3 mm²/s | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
300 °C | 9.3 mm²/s Show Material materials with Thermal diffusivity of 9.3 mm²/s | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
400 °C | 8.3 mm²/s Show Material materials with Thermal diffusivity of 8.3 mm²/s | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
500 °C | 7 mm²/s Show Material materials with Thermal diffusivity of 7 mm²/s | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
600 °C | 5.7 mm²/s Show Material materials with Thermal diffusivity of 5.7 mm²/s | normalized and tempered (+NT) | EN 10028-4 | Flat |
Electrical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Electrical conductivity | 7 S/m Show Material materials with Electrical conductivity of 7 S/m | Predicted Value | ||||
Electrical resistivity | 20 °C | 2.45e-07 Ω·m Show Material materials with Electrical resistivity of 2.45e-07 Ω·m | normalized and tempered (+NT) | EN 10028-4 | Flat | |
100 °C | 2.94e-07 Ω·m Show Material materials with Electrical resistivity of 2.94e-07 Ω·m | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
200 °C | 3.69e-07 Ω·m Show Material materials with Electrical resistivity of 3.69e-07 Ω·m | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
300 °C | 4.59e-07 Ω·m Show Material materials with Electrical resistivity of 4.59e-07 Ω·m | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
400 °C | 5.58e-07 Ω·m Show Material materials with Electrical resistivity of 5.58e-07 Ω·m | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
500 °C | 6.79e-07 Ω·m Show Material materials with Electrical resistivity of 6.79e-07 Ω·m | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
600 °C | 8.13e-07 Ω·m Show Material materials with Electrical resistivity of 8.13e-07 Ω·m | normalized and tempered (+NT) | EN 10028-4 | Flat |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | 0.02 % Show Material materials with Aluminium of 0.02 % | normalized and tempered (+NT) | EN 10028-4 | Flat |
Carbon | 0.16 % Show Material materials with Carbon of 0.16 % | normalized and tempered (+NT) | EN 10028-4 | Flat |
Manganese | 0.85 - 1.7 % Show Material materials with Manganese of 0.85 - 1.7 % | normalized and tempered (+NT) | EN 10028-4 | Flat |
Nickel | 0.3 - 0.85 % Show Material materials with Nickel of 0.3 - 0.85 % | normalized and tempered (+NT) | EN 10028-4 | Flat |
Niobium | 0.05 % Show Material materials with Niobium of 0.05 % | normalized and tempered (+NT) | EN 10028-4 | Flat |
Phosphorus | 0.025 % Show Material materials with Phosphorus of 0.025 % | normalized and tempered (+NT) | EN 10028-4 | Flat |
Silicon | 0.5 % Show Material materials with Silicon of 0.5 % | normalized and tempered (+NT) | EN 10028-4 | Flat |
Sulfur | 0.01 % Show Material materials with Sulfur of 0.01 % | normalized and tempered (+NT) | EN 10028-4 | Flat |
Vanadium | 0.05 % Show Material materials with Vanadium of 0.05 % | normalized and tempered (+NT) | EN 10028-4 | Flat |
Technological properties
Property | ||
---|---|---|
Supplier Disclaimer | The given information is a rough description and some properties can depend on various factors such as product thickness. Please contact the supplier or refer to the related norm or standard for further information. |
Do you have a technical question or need more information about this material?