General
Property | Value | Comment |
---|---|---|
Density | 7.8 - 7.9 g/cm³ Show Material materials with Density of 7.8 - 7.9 g/cm³ | Typical for Low Carbon Steel |
Mechanical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elastic modulus | 200 - 215 GPa Show Material materials with Elastic modulus of 200 - 215 GPa | Typical for Low Carbon Steel | ||||
Elongation | 18.2 % Show Material materials with Elongation of 18.2 % | Predicted Value, A200 | ||||
19.3 % Show Material materials with Elongation of 19.3 % | Predicted Value, A80 | |||||
20.1 % Show Material materials with Elongation of 20.1 % | Predicted Value, A80 Transverse | |||||
21.2 % Show Material materials with Elongation of 21.2 % | Predicted Value, A5 | |||||
22.6 % Show Material materials with Elongation of 22.6 % | Predicted Value, Transverse | |||||
25.5 % Show Material materials with Elongation of 25.5 % | Predicted Value, A50 | |||||
20 °C | 22 % Show Material materials with Elongation of 22 % | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Flat | ||
20 °C | 23 % Show Material materials with Elongation of 23 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 24 % Show Material materials with Elongation of 24 % | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat, Rod, Wire | ||
Hardness, Brinell | 243 [-] Show Material materials with Hardness, Brinell of 243 [-] | Predicted Value, Transverse | ||||
Poisson's ratio | 0.29 [-] Show Material materials with Poisson's ratio of 0.29 [-] | Typical for Low Carbon Steel | ||||
Reduction of area | 43.2 % Show Material materials with Reduction of area of 43.2 % | Predicted Value, Transverse | ||||
52.0 % Show Material materials with Reduction of area of 52.0 % | Predicted Value | |||||
Shear modulus | 82 GPa Show Material materials with Shear modulus of 82 GPa | Typical for Low Carbon Steel | ||||
Shear strength | 531 MPa Show Material materials with Shear strength of 531 MPa | Predicted Value | ||||
Tensile strength | 20 °C | 340 - 470 MPa Show Material materials with Tensile strength of 340 - 470 MPa | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Flat | |
20 °C | 350 - 510 MPa Show Material materials with Tensile strength of 350 - 510 MPa | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat, Rod, Wire | ||
20 °C | 350 - 480 MPa Show Material materials with Tensile strength of 350 - 480 MPa | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat, Rod, Wire | ||
20 °C | 370 - 510 MPa Show Material materials with Tensile strength of 370 - 510 MPa | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat, Rod, Wire | ||
20 °C | 370 - 480 MPa Show Material materials with Tensile strength of 370 - 480 MPa | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat, Rod, Wire | ||
Yield strength | 251.6 MPa Show Material materials with Yield strength of 251.6 MPa | Predicted Value, RP1 | ||||
317.2 MPa Show Material materials with Yield strength of 317.2 MPa | Predicted Value, RP02 | |||||
317.9 MPa Show Material materials with Yield strength of 317.9 MPa | Predicted Value, RP1 Transverse | |||||
319.8 MPa Show Material materials with Yield strength of 319.8 MPa | Predicted Value, Transverse | |||||
391.5 MPa Show Material materials with Yield strength of 391.5 MPa | Predicted Value, RP05 | |||||
453.7 MPa Show Material materials with Yield strength of 453.7 MPa | Predicted Value, RP002 | |||||
461.6 MPa Show Material materials with Yield strength of 461.6 MPa | Predicted Value, RP02 Transverse | |||||
20 °C | 205 MPa Show Material materials with Yield strength of 205 MPa | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 215 MPa Show Material materials with Yield strength of 215 MPa | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Flat, Strip, Rod, Wire | ||
20 °C | 225 MPa Show Material materials with Yield strength of 225 MPa | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat, Rod, Wire | ||
20 °C | 235 MPa Show Material materials with Yield strength of 235 MPa | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat, Rod, Wire | ||
20 °C | 245 MPa Show Material materials with Yield strength of 245 MPa | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat, Rod, Wire | ||
20 °C | 255 MPa Show Material materials with Yield strength of 255 MPa | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat, Rod, Wire | ||
20 °C | 265 MPa Show Material materials with Yield strength of 265 MPa | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat, Rod, Wire | ||
20 °C | 275 MPa Show Material materials with Yield strength of 275 MPa | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat, Rod, Wire |
Thermal
Property | Value | Comment |
---|---|---|
Coefficient of thermal expansion | 1.32e-05 - 1.38e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.32e-05 - 1.38e-05 1/K | Typical for Low Carbon Steel |
Max service temperature | 332 °C Show Material materials with Max service temperature of 332 °C | Predicted Value, Long |
500 °C Show Material materials with Max service temperature of 500 °C | Typical for Carbon Steel | |
Melting point | 1480 - 1526 °C Show Material materials with Melting point of 1480 - 1526 °C | Typical for Low Carbon Steel |
Specific heat capacity | 465 J/(kg·K) Show Material materials with Specific heat capacity of 465 J/(kg·K) | Typical for Low Carbon Steel |
Thermal conductivity | 25 - 93 W/(m·K) Show Material materials with Thermal conductivity of 25 - 93 W/(m·K) | Typical for Low Carbon Steel |
Electrical
Property | Value | Comment |
---|---|---|
Electrical conductivity | 6 S/m Show Material materials with Electrical conductivity of 6 S/m | Predicted Value |
Electrical resistivity | 1.43e-07 - 1.74e-07 Ω·m Show Material materials with Electrical resistivity of 1.43e-07 - 1.74e-07 Ω·m | Typical for Carbon Steel |
Magnetic
Property | Value | Comment |
---|---|---|
Curie temperature | 770 °C Show Material materials with Curie temperature of 770 °C | Typical for Low Carbon Steel |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | 0.02 % Show Material materials with Aluminium of 0.02 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar |
Carbon | 0.18 % Show Material materials with Carbon of 0.18 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar |
Chromium | 0.3 % Show Material materials with Chromium of 0.3 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar |
Copper | 0.35 % Show Material materials with Copper of 0.35 % | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat |
0.55 % Show Material materials with Copper of 0.55 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire | |
Manganese | 0.5 - 1.5 % Show Material materials with Manganese of 0.5 - 1.5 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire |
0.5 - 1.4 % Show Material materials with Manganese of 0.5 - 1.4 % | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat | |
Molybdenum | 0.1 % Show Material materials with Molybdenum of 0.1 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar |
Nickel | 0.3 % Show Material materials with Nickel of 0.3 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar |
Niobium | 0.05 % Show Material materials with Niobium of 0.05 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar |
Nitrogen | 0.015 % Show Material materials with Nitrogen of 0.015 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar |
Phosphorus | 0.03 % Show Material materials with Phosphorus of 0.03 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire |
0.035 % Show Material materials with Phosphorus of 0.035 % | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat | |
Silicon | 0.4 % Show Material materials with Silicon of 0.4 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar |
Sulfur | 0.025 % Show Material materials with Sulfur of 0.025 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire |
0.03 % Show Material materials with Sulfur of 0.03 % | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat | |
Titanium | 0.03 % Show Material materials with Titanium of 0.03 % | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat |
0.05 % Show Material materials with Titanium of 0.05 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire | |
Vanadium | 0.05 % Show Material materials with Vanadium of 0.05 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar |
Technological properties
Property | ||
---|---|---|
Supplier Disclaimer | The given information is a rough description and some properties can depend on various factors such as product thickness. Please contact the supplier or refer to the related norm or standard for further information. |