General
Property | Value | Comment |
---|---|---|
Density | 7.8 g/cm³ Show Material materials with Density of 7.8 g/cm³ | Typical for Steel |
Mechanical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elastic modulus | 190 - 210 GPa Show Material materials with Elastic modulus of 190 - 210 GPa | Typical for Steel | ||||
Elongation | 18.1 % Show Material materials with Elongation of 18.1 % | Predicted Value, A200 | ||||
20.1 % Show Material materials with Elongation of 20.1 % | Predicted Value, A80 | |||||
20.5 % Show Material materials with Elongation of 20.5 % | Predicted Value, A80 Transverse | |||||
21.0 % Show Material materials with Elongation of 21.0 % | Predicted Value, A5 | |||||
23.2 % Show Material materials with Elongation of 23.2 % | Predicted Value, Transverse | |||||
24.4 % Show Material materials with Elongation of 24.4 % | Predicted Value, A50 | |||||
20 °C | 24 % Show Material materials with Elongation of 24 % | thermomechanically rolled | EN 10113-3, EN 10025-4 | Sheet, Strip, Bar, Flat, Rod, Wire | ||
Hardness, Brinell | 243 [-] Show Material materials with Hardness, Brinell of 243 [-] | Predicted Value, Transverse | ||||
Poisson's ratio | 0.3 [-] Show Material materials with Poisson's ratio of 0.3 [-] | Typical for Steel | ||||
Reduction of area | 43.2 % Show Material materials with Reduction of area of 43.2 % | Predicted Value | ||||
44.2 % Show Material materials with Reduction of area of 44.2 % | Predicted Value, Transverse | |||||
Shear modulus | 80.1 GPa Show Material materials with Shear modulus of 80.1 GPa | Predicted Value | ||||
Shear strength | 532.6 MPa Show Material materials with Shear strength of 532.6 MPa | Predicted Value | ||||
Tensile strength | 20 °C | 350 - 530 MPa Show Material materials with Tensile strength of 350 - 530 MPa | thermomechanically rolled | EN 10025-4, EN 10113-3 | Strip, Sheet, Flat, Rod, Wire | |
20 °C | 350 - 523 MPa Show Material materials with Tensile strength of 350 - 523 MPa | thermomechanically rolled | EN 10025-4, EN 10113-3 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 350 - 510 MPa Show Material materials with Tensile strength of 350 - 510 MPa | thermomechanically rolled | EN 10025-4, EN 10113-3 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 360 - 510 MPa Show Material materials with Tensile strength of 360 - 510 MPa | thermomechanically rolled | EN 10113-3, EN 10025-4 | Sheet, Strip, Bar, Flat, Rod, Wire | ||
20 °C | 360 - 530 MPa Show Material materials with Tensile strength of 360 - 530 MPa | thermomechanically rolled | EN 10025-4, EN 10113-3 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 360 - 523 MPa Show Material materials with Tensile strength of 360 - 523 MPa | thermomechanically rolled | EN 10025-4, EN 10113-3 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 370 - 530 MPa Show Material materials with Tensile strength of 370 - 530 MPa | thermomechanically rolled | EN 10025-4, EN 10113-3 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 370 - 523 MPa Show Material materials with Tensile strength of 370 - 523 MPa | thermomechanically rolled | EN 10025-4, EN 10113-3 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 370 - 510 MPa Show Material materials with Tensile strength of 370 - 510 MPa | thermomechanically rolled | EN 10025-4, EN 10113-3 | Strip, Sheet, Flat, Rod, Wire | ||
Yield strength | 251.4 MPa Show Material materials with Yield strength of 251.4 MPa | Predicted Value, RP1 | ||||
318.6 MPa Show Material materials with Yield strength of 318.6 MPa | Predicted Value, RP1 Transverse | |||||
332.8 MPa Show Material materials with Yield strength of 332.8 MPa | Predicted Value, RP02 | |||||
360.5 MPa Show Material materials with Yield strength of 360.5 MPa | Predicted Value, Transverse | |||||
417.8 MPa Show Material materials with Yield strength of 417.8 MPa | Predicted Value, RP05 | |||||
464.9 MPa Show Material materials with Yield strength of 464.9 MPa | Predicted Value, RP02 Transverse | |||||
485 MPa Show Material materials with Yield strength of 485 MPa | Predicted Value, RP002 | |||||
20 °C | 240 MPa Show Material materials with Yield strength of 240 MPa | thermomechanically rolled | EN 10025-4, EN 10113-3 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 245 MPa Show Material materials with Yield strength of 245 MPa | thermomechanically rolled | EN 10025-4, EN 10113-3 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 255 MPa Show Material materials with Yield strength of 255 MPa | thermomechanically rolled | EN 10113-3, EN 10025-4 | Sheet, Strip, Bar, Flat, Rod, Wire | ||
20 °C | 265 MPa Show Material materials with Yield strength of 265 MPa | thermomechanically rolled | EN 10113-3, EN 10025-4 | Sheet, Strip, Bar, Flat, Rod, Wire | ||
20 °C | 275 MPa Show Material materials with Yield strength of 275 MPa | thermomechanically rolled | EN 10113-3, EN 10025-4 | Sheet, Strip, Bar, Flat, Rod, Wire |
Thermal
Property | Value | Comment |
---|---|---|
Coefficient of thermal expansion | 11.87 1/K Show Material materials with Coefficient of thermal expansion of 11.87 1/K | Predicted Value |
Specific heat capacity | 456.3 J/(kg·K) Show Material materials with Specific heat capacity of 456.3 J/(kg·K) | Predicted Value |
Thermal conductivity | 38.18 W/(m·K) Show Material materials with Thermal conductivity of 38.18 W/(m·K) | Predicted Value |
Electrical
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | 0.02 % Show Material materials with Aluminium of 0.02 % | thermomechanically rolled | EN 10113-3, EN 10025-4 | Sheet, Strip, Bar, Flat, Rod, Wire |
Carbon | 0.13 % Show Material materials with Carbon of 0.13 % | thermomechanically rolled | EN 10113-3, EN 10025-4 | Sheet, Strip, Bar, Flat, Rod, Wire |
Chromium | 0.3 % Show Material materials with Chromium of 0.3 % | thermomechanically rolled | EN 10025-4, EN 10113-3 | Strip, Sheet, Flat, Rod, Wire |
Copper | 0.55 % Show Material materials with Copper of 0.55 % | thermomechanically rolled | EN 10025-4, EN 10113-3 | Strip, Sheet, Flat, Rod, Wire |
Manganese | 1.5 % Show Material materials with Manganese of 1.5 % | thermomechanically rolled | EN 10113-3, EN 10025-4 | Sheet, Strip, Bar, Flat, Rod, Wire |
Molybdenum | 0.1 % Show Material materials with Molybdenum of 0.1 % | thermomechanically rolled | EN 10025-4, EN 10113-3 | Strip, Sheet, Flat, Rod, Wire |
0.2 % Show Material materials with Molybdenum of 0.2 % | thermomechanically rolled | EN 10113-3, EN 10025-4 | Sheet, Strip, Bar | |
Nickel | 0.3 % Show Material materials with Nickel of 0.3 % | thermomechanically rolled | EN 10113-3, EN 10025-4 | Sheet, Strip, Bar, Flat, Rod, Wire |
Niobium | 0.05 % Show Material materials with Niobium of 0.05 % | thermomechanically rolled | EN 10113-3, EN 10025-4 | Sheet, Strip, Bar, Flat, Rod, Wire |
Nitrogen | 0.015 % Show Material materials with Nitrogen of 0.015 % | thermomechanically rolled | EN 10113-3, EN 10025-4 | Sheet, Strip, Bar, Flat, Rod, Wire |
Phosphorus | 0.025 % Show Material materials with Phosphorus of 0.025 % | thermomechanically rolled | EN 10025-4, EN 10113-3 | Strip, Sheet, Flat, Rod, Wire |
0.03 % Show Material materials with Phosphorus of 0.03 % | thermomechanically rolled | EN 10113-3, EN 10025-4 | Sheet, Strip, Bar | |
Silicon | 0.5 % Show Material materials with Silicon of 0.5 % | thermomechanically rolled | EN 10113-3, EN 10025-4 | Sheet, Strip, Bar, Flat, Rod, Wire |
Sulfur | 0.02 % Show Material materials with Sulfur of 0.02 % | thermomechanically rolled | EN 10025-4, EN 10113-3 | Strip, Sheet, Flat, Rod, Wire |
0.025 % Show Material materials with Sulfur of 0.025 % | thermomechanically rolled | EN 10113-3, EN 10025-4 | Sheet, Strip, Bar | |
Titanium | 0.05 % Show Material materials with Titanium of 0.05 % | thermomechanically rolled | EN 10113-3, EN 10025-4 | Sheet, Strip, Bar, Flat, Rod, Wire |
Vanadium | 0.08 % Show Material materials with Vanadium of 0.08 % | thermomechanically rolled | EN 10113-3, EN 10025-4 | Sheet, Strip, Bar, Flat, Rod, Wire |
Technological properties
Property | ||
---|---|---|
Supplier Disclaimer | The given information is a rough description and some properties can depend on various factors such as product thickness. Please contact the supplier or refer to the related norm or standard for further information. |