EN 10028-7 Grade X2CrNi12 soft annealed (+A)

Want to keep this datasheet? Save it now in your required format

Description

The material X2CrNi12 is an ferritic steel of considerably higher corrosion resistance than general construction steels, but more cost-efficient than high-alloyed stainless steels. The corrosion resistance is comparable to the one of 13% Cr-steels. X2CrNi12 is unsuitable for higher corrosion requirements. Beside its sufficient corrosion resistance and favorable abrasion resistance the steel shows high static and dynamic strength values and ease of workability. Its not resistant to intercrystalline corrosion. Application: in transportation (construction of busses and containers), in agrarian and conveying engineering, civil engineering, e.g. for frameworks and front elements as well as in the mechanical and apparatus engineering

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

7.7 - 7.77 g/cm³

Show Material materials with Density of 7.7 - 7.77 g/cm³

Mechanical

PropertyTemperatureValue

Elastic modulus

20.0 °C

211.67 - 220 GPa

Show Material materials with Elastic modulus of 211.67 - 220 GPa

100.0 °C

213 - 215 GPa

Show Material materials with Elastic modulus of 213 - 215 GPa

200.0 °C

206 - 210 GPa

Show Material materials with Elastic modulus of 206 - 210 GPa

300.0 °C

198 - 205 GPa

Show Material materials with Elastic modulus of 198 - 205 GPa

400.0 °C

190 - 195 GPa

Show Material materials with Elastic modulus of 190 - 195 GPa

500.0 °C

180 GPa

Show Material materials with Elastic modulus of 180 GPa

600.0 °C

167 GPa

Show Material materials with Elastic modulus of 167 GPa

700.0 °C

150 GPa

Show Material materials with Elastic modulus of 150 GPa

Elongation

20.0 °C

18 - 20 %

Show Material materials with Elongation of 18 - 20 %

Elongation A80

20.0 °C

18 - 20 %

Show Material materials with Elongation A80 of 18 - 20 %

Elongation A80, transverse

20.0 °C

18 - 20 %

Show Material materials with Elongation A80, transverse of 18 - 20 %

Elongation, transverse

20.0 °C

18 - 20 %

Show Material materials with Elongation, transverse of 18 - 20 %

Poisson's ratio

20.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

Shear modulus

20.0 °C

81.7 GPa

Show Material materials with Shear modulus of 81.7 GPa

Tensile strength

20.0 °C

450 - 650 MPa

Show Material materials with Tensile strength of 450 - 650 MPa

Tensile strength, transverse

20.0 °C

450 - 650 MPa

Show Material materials with Tensile strength, transverse of 450 - 650 MPa

Yield strength Rp0.2

20.0 °C

250 - 280 MPa

Show Material materials with Yield strength Rp0.2 of 250 - 280 MPa

100.0 °C

240 MPa

Show Material materials with Yield strength Rp0.2 of 240 MPa

150.0 °C

235 MPa

Show Material materials with Yield strength Rp0.2 of 235 MPa

200.0 °C

230 MPa

Show Material materials with Yield strength Rp0.2 of 230 MPa

250.0 °C

220 MPa

Show Material materials with Yield strength Rp0.2 of 220 MPa

300.0 °C

215 MPa

Show Material materials with Yield strength Rp0.2 of 215 MPa

Unlock all property charts

Yield strength Rp0.2, transverse

20.0 °C

280 - 320 MPa

Show Material materials with Yield strength Rp0.2, transverse of 280 - 320 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

-100.0 °C

1E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1E-5 1/K

20.0 °C

1.08E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.08E-5 1/K

100.0 °C

1.04E-5 - 1.13E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.04E-5 - 1.13E-5 1/K

200.0 °C

1.08E-5 - 1.18E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.08E-5 - 1.18E-5 1/K

300.0 °C

1.12E-5 - 1.23E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.12E-5 - 1.23E-5 1/K

400.0 °C

1.16E-5 - 1.27E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.16E-5 - 1.27E-5 1/K

500.0 °C

1.19E-5 - 1.3E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.19E-5 - 1.3E-5 1/K

600.0 °C

1.32E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.32E-5 1/K

700.0 °C

1.33E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.33E-5 1/K

Unlock all property charts

Melting point

1425 - 1530 °C

Show Material materials with Melting point of 1425 - 1530 °C

Typical for Ferritic Stainless Steel

Specific heat capacity

20.0 °C

429 - 430 J/(kg·K)

Show Material materials with Specific heat capacity of 429 - 430 J/(kg·K)

100.0 °C

464 J/(kg·K)

Show Material materials with Specific heat capacity of 464 J/(kg·K)

200.0 °C

492 J/(kg·K)

Show Material materials with Specific heat capacity of 492 J/(kg·K)

300.0 °C

511 J/(kg·K)

Show Material materials with Specific heat capacity of 511 J/(kg·K)

400.0 °C

531 J/(kg·K)

Show Material materials with Specific heat capacity of 531 J/(kg·K)

500.0 °C

554 J/(kg·K)

Show Material materials with Specific heat capacity of 554 J/(kg·K)

600.0 °C

585 J/(kg·K)

Show Material materials with Specific heat capacity of 585 J/(kg·K)

700.0 °C

626 J/(kg·K)

Show Material materials with Specific heat capacity of 626 J/(kg·K)

Unlock all property charts

Thermal conductivity

20.0 °C

20.7 - 25 W/(m·K)

Show Material materials with Thermal conductivity of 20.7 - 25 W/(m·K)

100.0 °C

22.6 W/(m·K)

Show Material materials with Thermal conductivity of 22.6 W/(m·K)

200.0 °C

24.4 W/(m·K)

Show Material materials with Thermal conductivity of 24.4 W/(m·K)

300.0 °C

25.8 W/(m·K)

Show Material materials with Thermal conductivity of 25.8 W/(m·K)

400.0 °C

26.9 W/(m·K)

Show Material materials with Thermal conductivity of 26.9 W/(m·K)

500.0 °C

27.8 W/(m·K)

Show Material materials with Thermal conductivity of 27.8 W/(m·K)

600.0 °C

28.5 W/(m·K)

Show Material materials with Thermal conductivity of 28.5 W/(m·K)

700.0 °C

28.8 W/(m·K)

Show Material materials with Thermal conductivity of 28.8 W/(m·K)

Unlock all property charts

Thermal diffusivity

20.0 °C

6.2 mm²/s

Show Material materials with Thermal diffusivity of 6.2 mm²/s

100.0 °C

5.9 mm²/s

Show Material materials with Thermal diffusivity of 5.9 mm²/s

200.0 °C

6 mm²/s

Show Material materials with Thermal diffusivity of 6 mm²/s

300.0 °C

6 mm²/s

Show Material materials with Thermal diffusivity of 6 mm²/s

400.0 °C

5.7 mm²/s

Show Material materials with Thermal diffusivity of 5.7 mm²/s

500.0 °C

5.4 mm²/s

Show Material materials with Thermal diffusivity of 5.4 mm²/s

600.0 °C

4.8 mm²/s

Show Material materials with Thermal diffusivity of 4.8 mm²/s

700.0 °C

4 mm²/s

Show Material materials with Thermal diffusivity of 4 mm²/s

Unlock all property charts

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

5.03E-7 - 6E-7 Ω·m

Show Material materials with Electrical resistivity of 5.03E-7 - 6E-7 Ω·m

100.0 °C

5.67E-7 Ω·m

Show Material materials with Electrical resistivity of 5.67E-7 Ω·m

200.0 °C

6.47E-7 Ω·m

Show Material materials with Electrical resistivity of 6.47E-7 Ω·m

300.0 °C

7.27E-7 Ω·m

Show Material materials with Electrical resistivity of 7.27E-7 Ω·m

400.0 °C

8.09E-7 Ω·m

Show Material materials with Electrical resistivity of 8.09E-7 Ω·m

500.0 °C

8.9E-7 Ω·m

Show Material materials with Electrical resistivity of 8.9E-7 Ω·m

600.0 °C

9.72E-7 Ω·m

Show Material materials with Electrical resistivity of 9.72E-7 Ω·m

700.0 °C

1.06E-6 Ω·m

Show Material materials with Electrical resistivity of 1.06E-6 Ω·m

Unlock all property charts

Chemical properties

PropertyValue

Carbon

0.03 %

Show Material materials with Carbon of 0.03 %

Chromium

10.5 - 12.5 %

Show Material materials with Chromium of 10.5 - 12.5 %

Manganese

1.5 %

Show Material materials with Manganese of 1.5 %

Nickel

0.3 - 1 %

Show Material materials with Nickel of 0.3 - 1 %

Nitrogen

0.03 %

Show Material materials with Nitrogen of 0.03 %

Phosphorus

0.04 %

Show Material materials with Phosphorus of 0.04 %

Silicon

1 %

Show Material materials with Silicon of 1 %

Sulfur

0.015 %

Show Material materials with Sulfur of 0.015 %