EN 10028-7 Grade X5CrNi18-10 solution annealed (+AT)

Want to keep this datasheet? Save it now in your required format

Description

The basic type of the austenitic CrNi-steels X5CrNi18-10 shows high corrosion resistance but no resistance to intercrystalline corrosion in sensitized condition as well as favorable workability. The steel is suitable for mirror-polishing, is well cold formable, weldable and wear resistant. Application for welded parts in chemical apparatus engineering, food and milk industry, for household appliances, in breweries, in architecture and vehicle manufacturing as well as for pumps, compressors, instruments. Application also in water and low contaminated sewages. In pressure vessel construction up to 300 °C, above subject to authorization. The sort is acc. to DIN EN 10095 allowed to be used as a heat-resistant steel. Application temperature: -200 to 550 °C. In construction trade X5CrNi18-10 is applicated for decorative purposes in exterior and interior architecture, e.g. roof and wall elements, facings, washing plants, washbasins in toilets, for doors and windows. The material is approved for structural components (extended approval certificate Nr. Z-30.44.1 of Institut für Bautechnik Berlin, dated 01/02/89, containing demands for materials, calculation, construction and control). Strength grades E 225 and E 355 are common.

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

7.9 - 7.92 g/cm³

Show Material materials with Density of 7.9 - 7.92 g/cm³

Mechanical

PropertyTemperatureValue

Elastic modulus

-100.0 °C

206 GPa

Show Material materials with Elastic modulus of 206 GPa

20.0 °C

196 - 200 GPa

Show Material materials with Elastic modulus of 196 - 200 GPa

24.0 °C

194.4 - 196.5 GPa

Show Material materials with Elastic modulus of 194.4 - 196.5 GPa

100.0 °C

190 - 194 GPa

Show Material materials with Elastic modulus of 190 - 194 GPa

149.0 °C

188.2 - 189.6 GPa

Show Material materials with Elastic modulus of 188.2 - 189.6 GPa

200.0 °C

182 - 186 GPa

Show Material materials with Elastic modulus of 182 - 186 GPa

260.0 °C

182.7 - 184.1 GPa

Show Material materials with Elastic modulus of 182.7 - 184.1 GPa

300.0 °C

174 - 179 GPa

Show Material materials with Elastic modulus of 174 - 179 GPa

371.0 °C

173.1 - 177.9 GPa

Show Material materials with Elastic modulus of 173.1 - 177.9 GPa

400.0 °C

166 - 172 GPa

Show Material materials with Elastic modulus of 166 - 172 GPa

483.0 °C

157.9 - 160 GPa

Show Material materials with Elastic modulus of 157.9 - 160 GPa

500.0 °C

158 - 165 GPa

Show Material materials with Elastic modulus of 158 - 165 GPa

593.0 °C

149.6 - 155.8 GPa

Show Material materials with Elastic modulus of 149.6 - 155.8 GPa

600.0 °C

150 GPa

Show Material materials with Elastic modulus of 150 GPa

700.0 °C

142 GPa

Show Material materials with Elastic modulus of 142 GPa

704.0 °C

137.9 - 144.8 GPa

Show Material materials with Elastic modulus of 137.9 - 144.8 GPa

800.0 °C

134 GPa

Show Material materials with Elastic modulus of 134 GPa

816.0 °C

120.7 - 128.2 GPa

Show Material materials with Elastic modulus of 120.7 - 128.2 GPa

Elongation

-196.0 °C

30 %

Show Material materials with Elongation of 30 %

-150.0 °C

30 %

Show Material materials with Elongation of 30 %

-80.0 °C

35 %

Show Material materials with Elongation of 35 %

20.0 °C

45 %

Show Material materials with Elongation of 45 %

Unlock all property charts

Elongation A80, transverse

20.0 °C

45 %

Show Material materials with Elongation A80, transverse of 45 %

Elongation, transverse

20.0 °C

45 %

Show Material materials with Elongation, transverse of 45 %

Poisson's ratio

20.0 °C

0.28 [-]

Show Material materials with Poisson's ratio of 0.28 [-]

24.0 °C

0.24 - 0.25 [-]

Show Material materials with Poisson's ratio of 0.24 - 0.25 [-]

149.0 °C

0.27 - 0.3 [-]

Show Material materials with Poisson's ratio of 0.27 - 0.3 [-]

260.0 °C

0.29 - 0.32 [-]

Show Material materials with Poisson's ratio of 0.29 - 0.32 [-]

371.0 °C

0.32 [-]

Show Material materials with Poisson's ratio of 0.32 [-]

483.0 °C

0.27 - 0.29 [-]

Show Material materials with Poisson's ratio of 0.27 - 0.29 [-]

593.0 °C

0.29 - 0.3 [-]

Show Material materials with Poisson's ratio of 0.29 - 0.3 [-]

704.0 °C

0.27 - 0.3 [-]

Show Material materials with Poisson's ratio of 0.27 - 0.3 [-]

816.0 °C

0.23 - 0.27 [-]

Show Material materials with Poisson's ratio of 0.23 - 0.27 [-]

Unlock all property charts

Shear modulus

24.0 °C

78.6 GPa

Show Material materials with Shear modulus of 78.6 GPa

149.0 °C

72.4 - 74.5 GPa

Show Material materials with Shear modulus of 72.4 - 74.5 GPa

260.0 °C

69.6 - 71 GPa

Show Material materials with Shear modulus of 69.6 - 71 GPa

371.0 °C

65.5 - 67.6 GPa

Show Material materials with Shear modulus of 65.5 - 67.6 GPa

483.0 °C

62.1 GPa

Show Material materials with Shear modulus of 62.1 GPa

593.0 °C

57.9 - 60 GPa

Show Material materials with Shear modulus of 57.9 - 60 GPa

704.0 °C

54.5 - 55.9 GPa

Show Material materials with Shear modulus of 54.5 - 55.9 GPa

816.0 °C

49 - 50.3 GPa

Show Material materials with Shear modulus of 49 - 50.3 GPa

Unlock all property charts

Tensile strength

-196.0 °C

1250 MPa

Show Material materials with Tensile strength of 1250 MPa

-150.0 °C

1100 MPa

Show Material materials with Tensile strength of 1100 MPa

-80.0 °C

860 MPa

Show Material materials with Tensile strength of 860 MPa

20.0 °C

520 - 750 MPa

Show Material materials with Tensile strength of 520 - 750 MPa

50.0 °C

494 MPa

Show Material materials with Tensile strength of 494 MPa

100.0 °C

450 MPa

Show Material materials with Tensile strength of 450 MPa

150.0 °C

420 MPa

Show Material materials with Tensile strength of 420 MPa

200.0 °C

400 MPa

Show Material materials with Tensile strength of 400 MPa

250.0 °C

390 MPa

Show Material materials with Tensile strength of 390 MPa

300.0 °C

380 MPa

Show Material materials with Tensile strength of 380 MPa

350.0 °C

380 MPa

Show Material materials with Tensile strength of 380 MPa

400.0 °C

380 MPa

Show Material materials with Tensile strength of 380 MPa

450.0 °C

370 MPa

Show Material materials with Tensile strength of 370 MPa

500.0 °C

360 MPa

Show Material materials with Tensile strength of 360 MPa

550.0 °C

330 MPa

Show Material materials with Tensile strength of 330 MPa

Unlock all property charts

Tensile strength, transverse

20.0 °C

520 - 750 MPa

Show Material materials with Tensile strength, transverse of 520 - 750 MPa

Yield strength Rp0.2

-196.0 °C

300 MPa

Show Material materials with Yield strength Rp0.2 of 300 MPa

-150.0 °C

315 MPa

Show Material materials with Yield strength Rp0.2 of 315 MPa

-80.0 °C

270 MPa

Show Material materials with Yield strength Rp0.2 of 270 MPa

20.0 °C

210 MPa

Show Material materials with Yield strength Rp0.2 of 210 MPa

50.0 °C

190 MPa

Show Material materials with Yield strength Rp0.2 of 190 MPa

100.0 °C

157 MPa

Show Material materials with Yield strength Rp0.2 of 157 MPa

150.0 °C

142 MPa

Show Material materials with Yield strength Rp0.2 of 142 MPa

200.0 °C

127 MPa

Show Material materials with Yield strength Rp0.2 of 127 MPa

250.0 °C

118 MPa

Show Material materials with Yield strength Rp0.2 of 118 MPa

300.0 °C

110 MPa

Show Material materials with Yield strength Rp0.2 of 110 MPa

350.0 °C

104 MPa

Show Material materials with Yield strength Rp0.2 of 104 MPa

400.0 °C

98 MPa

Show Material materials with Yield strength Rp0.2 of 98 MPa

450.0 °C

95 MPa

Show Material materials with Yield strength Rp0.2 of 95 MPa

500.0 °C

92 MPa

Show Material materials with Yield strength Rp0.2 of 92 MPa

550.0 °C

90 MPa

Show Material materials with Yield strength Rp0.2 of 90 MPa

Unlock all property charts

Yield strength Rp0.2, transverse

20.0 °C

210 - 230 MPa

Show Material materials with Yield strength Rp0.2, transverse of 210 - 230 MPa

Yield strength Rp1.0

-196.0 °C

400 MPa

Show Material materials with Yield strength Rp1.0 of 400 MPa

-150.0 °C

415 MPa

Show Material materials with Yield strength Rp1.0 of 415 MPa

-80.0 °C

350 MPa

Show Material materials with Yield strength Rp1.0 of 350 MPa

20.0 °C

250 MPa

Show Material materials with Yield strength Rp1.0 of 250 MPa

50.0 °C

228 MPa

Show Material materials with Yield strength Rp1.0 of 228 MPa

100.0 °C

191 MPa

Show Material materials with Yield strength Rp1.0 of 191 MPa

150.0 °C

172 MPa

Show Material materials with Yield strength Rp1.0 of 172 MPa

200.0 °C

157 MPa

Show Material materials with Yield strength Rp1.0 of 157 MPa

250.0 °C

145 MPa

Show Material materials with Yield strength Rp1.0 of 145 MPa

300.0 °C

135 MPa

Show Material materials with Yield strength Rp1.0 of 135 MPa

350.0 °C

129 MPa

Show Material materials with Yield strength Rp1.0 of 129 MPa

400.0 °C

125 MPa

Show Material materials with Yield strength Rp1.0 of 125 MPa

450.0 °C

122 MPa

Show Material materials with Yield strength Rp1.0 of 122 MPa

500.0 °C

120 MPa

Show Material materials with Yield strength Rp1.0 of 120 MPa

550.0 °C

120 MPa

Show Material materials with Yield strength Rp1.0 of 120 MPa

Unlock all property charts

Yield strength Rp1.0, transverse

20.0 °C

250 - 260 MPa

Show Material materials with Yield strength Rp1.0, transverse of 250 - 260 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

-100.0 °C

1.49E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.49E-5 1/K

20.0 °C

1.61E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.61E-5 1/K

100.0 °C

1.6E-5 - 1.67E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.6E-5 - 1.67E-5 1/K

200.0 °C

1.65E-5 - 1.72E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.65E-5 - 1.72E-5 1/K

300.0 °C

1.7E-5 - 1.77E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.7E-5 - 1.77E-5 1/K

400.0 °C

1.75E-5 - 1.81E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.75E-5 - 1.81E-5 1/K

500.0 °C

1.8E-5 - 1.84E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.8E-5 - 1.84E-5 1/K

600.0 °C

1.88E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.88E-5 1/K

700.0 °C

1.91E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.91E-5 1/K

800.0 °C

1.94E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.94E-5 1/K

Unlock all property charts

Max service temperature, long

-200 - 550 °C

Show Material materials with Max service temperature, long of -200 - 550 °C

Melting point

1230 - 1480 °C

Show Material materials with Melting point of 1230 - 1480 °C

Typical for Austenitic Stainless Steel

Specific heat capacity

-100.0 °C

440 J/(kg·K)

Show Material materials with Specific heat capacity of 440 J/(kg·K)

20.0 °C

472 - 500 J/(kg·K)

Show Material materials with Specific heat capacity of 472 - 500 J/(kg·K)

100.0 °C

487 J/(kg·K)

Show Material materials with Specific heat capacity of 487 J/(kg·K)

200.0 °C

503 J/(kg·K)

Show Material materials with Specific heat capacity of 503 J/(kg·K)

300.0 °C

512 J/(kg·K)

Show Material materials with Specific heat capacity of 512 J/(kg·K)

400.0 °C

520 J/(kg·K)

Show Material materials with Specific heat capacity of 520 J/(kg·K)

500.0 °C

530 J/(kg·K)

Show Material materials with Specific heat capacity of 530 J/(kg·K)

600.0 °C

541 J/(kg·K)

Show Material materials with Specific heat capacity of 541 J/(kg·K)

700.0 °C

551 J/(kg·K)

Show Material materials with Specific heat capacity of 551 J/(kg·K)

800.0 °C

559 J/(kg·K)

Show Material materials with Specific heat capacity of 559 J/(kg·K)

Unlock all property charts

Thermal conductivity

-100.0 °C

11.7 W/(m·K)

Show Material materials with Thermal conductivity of 11.7 W/(m·K)

20.0 °C

14.5 - 15 W/(m·K)

Show Material materials with Thermal conductivity of 14.5 - 15 W/(m·K)

100.0 °C

16 W/(m·K)

Show Material materials with Thermal conductivity of 16 W/(m·K)

200.0 °C

17.6 W/(m·K)

Show Material materials with Thermal conductivity of 17.6 W/(m·K)

300.0 °C

19.1 W/(m·K)

Show Material materials with Thermal conductivity of 19.1 W/(m·K)

400.0 °C

20.4 W/(m·K)

Show Material materials with Thermal conductivity of 20.4 W/(m·K)

500.0 °C

21.9 W/(m·K)

Show Material materials with Thermal conductivity of 21.9 W/(m·K)

600.0 °C

23.3 W/(m·K)

Show Material materials with Thermal conductivity of 23.3 W/(m·K)

700.0 °C

24.7 W/(m·K)

Show Material materials with Thermal conductivity of 24.7 W/(m·K)

800.0 °C

26.1 W/(m·K)

Show Material materials with Thermal conductivity of 26.1 W/(m·K)

Unlock all property charts

Thermal diffusivity

-100.0 °C

3.7 mm²/s

Show Material materials with Thermal diffusivity of 3.7 mm²/s

20.0 °C

3.9 mm²/s

Show Material materials with Thermal diffusivity of 3.9 mm²/s

100.0 °C

4.3 mm²/s

Show Material materials with Thermal diffusivity of 4.3 mm²/s

200.0 °C

4.3 mm²/s

Show Material materials with Thermal diffusivity of 4.3 mm²/s

300.0 °C

4.6 mm²/s

Show Material materials with Thermal diffusivity of 4.6 mm²/s

400.0 °C

4.7 mm²/s

Show Material materials with Thermal diffusivity of 4.7 mm²/s

500.0 °C

4.9 mm²/s

Show Material materials with Thermal diffusivity of 4.9 mm²/s

600.0 °C

5 mm²/s

Show Material materials with Thermal diffusivity of 5 mm²/s

700.0 °C

5.3 mm²/s

Show Material materials with Thermal diffusivity of 5.3 mm²/s

800.0 °C

5.7 mm²/s

Show Material materials with Thermal diffusivity of 5.7 mm²/s

Unlock all property charts

Electrical

PropertyTemperatureValue

Electrical resistivity

-100.0 °C

5.86E-7 Ω·m

Show Material materials with Electrical resistivity of 5.86E-7 Ω·m

20.0 °C

6.92E-7 - 7.3E-7 Ω·m

Show Material materials with Electrical resistivity of 6.92E-7 - 7.3E-7 Ω·m

100.0 °C

7.58E-7 Ω·m

Show Material materials with Electrical resistivity of 7.58E-7 Ω·m

200.0 °C

8.36E-7 Ω·m

Show Material materials with Electrical resistivity of 8.36E-7 Ω·m

300.0 °C

9.07E-7 Ω·m

Show Material materials with Electrical resistivity of 9.07E-7 Ω·m

400.0 °C

9.73E-7 Ω·m

Show Material materials with Electrical resistivity of 9.73E-7 Ω·m

500.0 °C

1.02E-6 Ω·m

Show Material materials with Electrical resistivity of 1.02E-6 Ω·m

600.0 °C

1.06E-6 Ω·m

Show Material materials with Electrical resistivity of 1.06E-6 Ω·m

700.0 °C

1.1E-6 Ω·m

Show Material materials with Electrical resistivity of 1.1E-6 Ω·m

800.0 °C

1.13E-6 Ω·m

Show Material materials with Electrical resistivity of 1.13E-6 Ω·m

Unlock all property charts

Chemical properties

PropertyValue

Carbon

0.07 %

Show Material materials with Carbon of 0.07 %

Chromium

17 - 19.5 %

Show Material materials with Chromium of 17 - 19.5 %

Manganese

2 %

Show Material materials with Manganese of 2 %

Nickel

8 - 10.5 %

Show Material materials with Nickel of 8 - 10.5 %

Nitrogen

0.1 - 0.11 %

Show Material materials with Nitrogen of 0.1 - 0.11 %

Phosphorus

0.05 %

Show Material materials with Phosphorus of 0.05 %

Silicon

1 %

Show Material materials with Silicon of 1 %

Sulfur

0.015 %

Show Material materials with Sulfur of 0.015 %