Description

The heat resistant austenitic steel X8NiCrAlTi32-21 is optimized concerning high creep rupture strength at 700 to 1000 °C. The material is resistant to intercrystalline corrosion, not in the sensitized condition. Application: in pressure vessel and steam-boiler construction as well as in chemical and petrochemical industry

Related Standards

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

7.94 - 8 g/cm³

Show Material materials with Density of 7.94 - 8 g/cm³

Mechanical

PropertyTemperatureValueComment

Elastic modulus

-100.0 °C

201 GPa

Show Material materials with Elastic modulus of 201 GPa

20.0 °C

194 - 200 GPa

Show Material materials with Elastic modulus of 194 - 200 GPa

100.0 °C

189 - 190 GPa

Show Material materials with Elastic modulus of 189 - 190 GPa

200.0 °C

183 - 185 GPa

Show Material materials with Elastic modulus of 183 - 185 GPa

300.0 °C

175 - 177 GPa

Show Material materials with Elastic modulus of 175 - 177 GPa

400.0 °C

170 GPa

Show Material materials with Elastic modulus of 170 GPa

500.0 °C

160 - 163 GPa

Show Material materials with Elastic modulus of 160 - 163 GPa

600.0 °C

155 - 156 GPa

Show Material materials with Elastic modulus of 155 - 156 GPa

700.0 °C

145 - 149 GPa

Show Material materials with Elastic modulus of 145 - 149 GPa

800.0 °C

140 - 141 GPa

Show Material materials with Elastic modulus of 140 - 141 GPa

900.0 °C

134 - 135 GPa

Show Material materials with Elastic modulus of 134 - 135 GPa

1000.0 °C

125 - 127 GPa

Show Material materials with Elastic modulus of 125 - 127 GPa

Elongation A80, transverse

20.0 °C

30 %

Show Material materials with Elongation A80, transverse of 30 %

Elongation, transverse

20.0 °C

30 %

Show Material materials with Elongation, transverse of 30 %

Poisson's ratio

23.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

Typical for Austenitic Stainless Steel

Shear modulus

23.0 °C

77 GPa

Show Material materials with Shear modulus of 77 GPa

Typical for Austenitic Stainless Steel

Tensile strength

20.0 °C

500 - 750 MPa

Show Material materials with Tensile strength of 500 - 750 MPa

50.0 °C

487 MPa

Show Material materials with Tensile strength of 487 MPa

100.0 °C

465 MPa

Show Material materials with Tensile strength of 465 MPa

150.0 °C

445 MPa

Show Material materials with Tensile strength of 445 MPa

200.0 °C

435 MPa

Show Material materials with Tensile strength of 435 MPa

250.0 °C

425 MPa

Show Material materials with Tensile strength of 425 MPa

300.0 °C

420 MPa

Show Material materials with Tensile strength of 420 MPa

350.0 °C

418 MPa

Show Material materials with Tensile strength of 418 MPa

400.0 °C

415 MPa

Show Material materials with Tensile strength of 415 MPa

450.0 °C

415 MPa

Show Material materials with Tensile strength of 415 MPa

500.0 °C

415 MPa

Show Material materials with Tensile strength of 415 MPa

Unlock all property charts

Tensile strength, transverse

20.0 °C

500 - 750 MPa

Show Material materials with Tensile strength, transverse of 500 - 750 MPa

Yield strength Rp0.2

50.0 °C

159 MPa

Show Material materials with Yield strength Rp0.2 of 159 MPa

100.0 °C

140 MPa

Show Material materials with Yield strength Rp0.2 of 140 MPa

150.0 °C

127 MPa

Show Material materials with Yield strength Rp0.2 of 127 MPa

200.0 °C

115 MPa

Show Material materials with Yield strength Rp0.2 of 115 MPa

250.0 °C

105 MPa

Show Material materials with Yield strength Rp0.2 of 105 MPa

300.0 °C

95 MPa

Show Material materials with Yield strength Rp0.2 of 95 MPa

350.0 °C

90 MPa

Show Material materials with Yield strength Rp0.2 of 90 MPa

400.0 °C

85 MPa

Show Material materials with Yield strength Rp0.2 of 85 MPa

450.0 °C

82 MPa

Show Material materials with Yield strength Rp0.2 of 82 MPa

500.0 °C

80 MPa

Show Material materials with Yield strength Rp0.2 of 80 MPa

550.0 °C

75 MPa

Show Material materials with Yield strength Rp0.2 of 75 MPa

600.0 °C

75 MPa

Show Material materials with Yield strength Rp0.2 of 75 MPa

Unlock all property charts

Yield strength Rp0.2, transverse

20.0 °C

170 MPa

Show Material materials with Yield strength Rp0.2, transverse of 170 MPa

Yield strength Rp1.0

50.0 °C

185 MPa

Show Material materials with Yield strength Rp1.0 of 185 MPa

100.0 °C

160 MPa

Show Material materials with Yield strength Rp1.0 of 160 MPa

150.0 °C

147 MPa

Show Material materials with Yield strength Rp1.0 of 147 MPa

200.0 °C

135 MPa

Show Material materials with Yield strength Rp1.0 of 135 MPa

250.0 °C

125 MPa

Show Material materials with Yield strength Rp1.0 of 125 MPa

300.0 °C

115 MPa

Show Material materials with Yield strength Rp1.0 of 115 MPa

350.0 °C

110 MPa

Show Material materials with Yield strength Rp1.0 of 110 MPa

400.0 °C

105 MPa

Show Material materials with Yield strength Rp1.0 of 105 MPa

450.0 °C

102 MPa

Show Material materials with Yield strength Rp1.0 of 102 MPa

500.0 °C

100 MPa

Show Material materials with Yield strength Rp1.0 of 100 MPa

550.0 °C

95 MPa

Show Material materials with Yield strength Rp1.0 of 95 MPa

600.0 °C

95 MPa

Show Material materials with Yield strength Rp1.0 of 95 MPa

Unlock all property charts

Yield strength Rp1.0, transverse

20.0 °C

200 MPa

Show Material materials with Yield strength Rp1.0, transverse of 200 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

-100.0 °C

1.36E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.36E-5 1/K

20.0 °C

1.46E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.46E-5 1/K

100.0 °C

1.51E-5 - 1.54E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.51E-5 - 1.54E-5 1/K

200.0 °C

1.57E-5 - 1.6E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.57E-5 - 1.6E-5 1/K

300.0 °C

1.62E-5 - 1.65E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.62E-5 - 1.65E-5 1/K

400.0 °C

1.66E-5 - 1.68E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.66E-5 - 1.68E-5 1/K

500.0 °C

1.7E-5 - 1.72E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.7E-5 - 1.72E-5 1/K

600.0 °C

1.74E-5 - 1.75E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.74E-5 - 1.75E-5 1/K

700.0 °C

1.77E-5 - 1.79E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.77E-5 - 1.79E-5 1/K

800.0 °C

1.8E-5 - 1.83E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.8E-5 - 1.83E-5 1/K

900.0 °C

1.83E-5 - 1.86E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.83E-5 - 1.86E-5 1/K

1000.0 °C

1.86E-5 - 1.9E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.86E-5 - 1.9E-5 1/K

Unlock all property charts

Max service temperature, long

700 - 1000 °C

Show Material materials with Max service temperature, long of 700 - 1000 °C

Melting point

1230 - 1480 °C

Show Material materials with Melting point of 1230 - 1480 °C

Typical for Austenitic Stainless Steel

Specific heat capacity

-100.0 °C

440 J/(kg·K)

Show Material materials with Specific heat capacity of 440 J/(kg·K)

20.0 °C

460 - 472 J/(kg·K)

Show Material materials with Specific heat capacity of 460 - 472 J/(kg·K)

100.0 °C

487 J/(kg·K)

Show Material materials with Specific heat capacity of 487 J/(kg·K)

200.0 °C

503 J/(kg·K)

Show Material materials with Specific heat capacity of 503 J/(kg·K)

300.0 °C

512 J/(kg·K)

Show Material materials with Specific heat capacity of 512 J/(kg·K)

400.0 °C

520 J/(kg·K)

Show Material materials with Specific heat capacity of 520 J/(kg·K)

500.0 °C

530 J/(kg·K)

Show Material materials with Specific heat capacity of 530 J/(kg·K)

600.0 °C

541 J/(kg·K)

Show Material materials with Specific heat capacity of 541 J/(kg·K)

700.0 °C

551 J/(kg·K)

Show Material materials with Specific heat capacity of 551 J/(kg·K)

800.0 °C

559 J/(kg·K)

Show Material materials with Specific heat capacity of 559 J/(kg·K)

900.0 °C

565 J/(kg·K)

Show Material materials with Specific heat capacity of 565 J/(kg·K)

1000.0 °C

571 J/(kg·K)

Show Material materials with Specific heat capacity of 571 J/(kg·K)

Unlock all property charts

Thermal conductivity

20.0 °C

11.5 - 12 W/(m·K)

Show Material materials with Thermal conductivity of 11.5 - 12 W/(m·K)

100.0 °C

13.1 W/(m·K)

Show Material materials with Thermal conductivity of 13.1 W/(m·K)

200.0 °C

14.8 W/(m·K)

Show Material materials with Thermal conductivity of 14.8 W/(m·K)

300.0 °C

16.4 W/(m·K)

Show Material materials with Thermal conductivity of 16.4 W/(m·K)

400.0 °C

18.1 W/(m·K)

Show Material materials with Thermal conductivity of 18.1 W/(m·K)

500.0 °C

19.6 W/(m·K)

Show Material materials with Thermal conductivity of 19.6 W/(m·K)

600.0 °C

21.2 W/(m·K)

Show Material materials with Thermal conductivity of 21.2 W/(m·K)

700.0 °C

22.8 W/(m·K)

Show Material materials with Thermal conductivity of 22.8 W/(m·K)

800.0 °C

24.3 W/(m·K)

Show Material materials with Thermal conductivity of 24.3 W/(m·K)

900.0 °C

25.7 W/(m·K)

Show Material materials with Thermal conductivity of 25.7 W/(m·K)

1000.0 °C

27.3 W/(m·K)

Show Material materials with Thermal conductivity of 27.3 W/(m·K)

Unlock all property charts

Thermal diffusivity

20.0 °C

3.1 mm²/s

Show Material materials with Thermal diffusivity of 3.1 mm²/s

100.0 °C

3.3 mm²/s

Show Material materials with Thermal diffusivity of 3.3 mm²/s

200.0 °C

3.6 mm²/s

Show Material materials with Thermal diffusivity of 3.6 mm²/s

300.0 °C

3.9 mm²/s

Show Material materials with Thermal diffusivity of 3.9 mm²/s

400.0 °C

4.2 mm²/s

Show Material materials with Thermal diffusivity of 4.2 mm²/s

500.0 °C

4.4 mm²/s

Show Material materials with Thermal diffusivity of 4.4 mm²/s

600.0 °C

4.6 mm²/s

Show Material materials with Thermal diffusivity of 4.6 mm²/s

700.0 °C

4.9 mm²/s

Show Material materials with Thermal diffusivity of 4.9 mm²/s

800.0 °C

5.2 mm²/s

Show Material materials with Thermal diffusivity of 5.2 mm²/s

900.0 °C

5.5 mm²/s

Show Material materials with Thermal diffusivity of 5.5 mm²/s

1000.0 °C

5.7 mm²/s

Show Material materials with Thermal diffusivity of 5.7 mm²/s

Unlock all property charts

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

9.9E-7 - 1.01E-6 Ω·m

Show Material materials with Electrical resistivity of 9.9E-7 - 1.01E-6 Ω·m

100.0 °C

1.04E-6 Ω·m

Show Material materials with Electrical resistivity of 1.04E-6 Ω·m

200.0 °C

1.08E-6 Ω·m

Show Material materials with Electrical resistivity of 1.08E-6 Ω·m

300.0 °C

1.12E-6 Ω·m

Show Material materials with Electrical resistivity of 1.12E-6 Ω·m

400.0 °C

1.15E-6 Ω·m

Show Material materials with Electrical resistivity of 1.15E-6 Ω·m

500.0 °C

1.18E-6 Ω·m

Show Material materials with Electrical resistivity of 1.18E-6 Ω·m

600.0 °C

1.2E-6 Ω·m

Show Material materials with Electrical resistivity of 1.2E-6 Ω·m

700.0 °C

1.22E-6 Ω·m

Show Material materials with Electrical resistivity of 1.22E-6 Ω·m

800.0 °C

1.24E-6 Ω·m

Show Material materials with Electrical resistivity of 1.24E-6 Ω·m

900.0 °C

1.26E-6 Ω·m

Show Material materials with Electrical resistivity of 1.26E-6 Ω·m

1000.0 °C

1.27E-6 Ω·m

Show Material materials with Electrical resistivity of 1.27E-6 Ω·m

Unlock all property charts

Chemical properties

PropertyValue

Aluminium

0.25 - 0.65 %

Show Material materials with Aluminium of 0.25 - 0.65 %

Carbon

0.05 - 0.1 %

Show Material materials with Carbon of 0.05 - 0.1 %

Chromium

19 - 22 %

Show Material materials with Chromium of 19 - 22 %

Cobalt

0.5 %

Show Material materials with Cobalt of 0.5 %

Copper

0.5 %

Show Material materials with Copper of 0.5 %

Manganese

1.5 %

Show Material materials with Manganese of 1.5 %

Nickel

30 - 34 %

Show Material materials with Nickel of 30 - 34 %

Nitrogen

0.03 %

Show Material materials with Nitrogen of 0.03 %

Phosphorus

0.02 %

Show Material materials with Phosphorus of 0.02 %

Silicon

0.7 %

Show Material materials with Silicon of 0.7 %

Sulfur

0.01 %

Show Material materials with Sulfur of 0.01 %

Titanium

0.25 - 0.65 %

Show Material materials with Titanium of 0.25 - 0.65 %