General
Property | Temperature | Value |
---|---|---|
Density | 20.0 °C | 7.76 - 7.9 g/cm³ Show Material materials with Density of 7.76 - 7.9 g/cm³ |
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elastic modulus | -100.0 °C | 206 GPa Show Material materials with Elastic modulus of 206 GPa | |
20.0 °C | 195 - 196 GPa Show Material materials with Elastic modulus of 195 - 196 GPa | ||
100.0 °C | 190 GPa Show Material materials with Elastic modulus of 190 GPa | ||
200.0 °C | 182 GPa Show Material materials with Elastic modulus of 182 GPa | ||
300.0 °C | 174 GPa Show Material materials with Elastic modulus of 174 GPa | ||
400.0 °C | 166 GPa Show Material materials with Elastic modulus of 166 GPa | ||
500.0 °C | 158 GPa Show Material materials with Elastic modulus of 158 GPa | ||
600.0 °C | 150 GPa Show Material materials with Elastic modulus of 150 GPa | ||
700.0 °C | 142 GPa Show Material materials with Elastic modulus of 142 GPa | ||
800.0 °C | 134 GPa Show Material materials with Elastic modulus of 134 GPa | ||
900.0 °C | 127 GPa Show Material materials with Elastic modulus of 127 GPa | ||
1000.0 °C | 120 GPa Show Material materials with Elastic modulus of 120 GPa | ||
Elongation A80, transverse | 20.0 °C | 40 % Show Material materials with Elongation A80, transverse of 40 % | |
Elongation, transverse | 20.0 °C | 40 % Show Material materials with Elongation, transverse of 40 % | |
Poisson's ratio | 23.0 °C | 0.3 [-] Show Material materials with Poisson's ratio of 0.3 [-] | Typical for Austenitic Stainless Steel |
Shear modulus | 23.0 °C | 77 GPa Show Material materials with Shear modulus of 77 GPa | Typical for Austenitic Stainless Steel |
Tensile strength | 20.0 °C | 470 - 670 MPa Show Material materials with Tensile strength of 470 - 670 MPa | |
50.0 °C | 459 MPa Show Material materials with Tensile strength of 459 MPa | ||
100.0 °C | 440 MPa Show Material materials with Tensile strength of 440 MPa | ||
150.0 °C | 425 MPa Show Material materials with Tensile strength of 425 MPa | ||
200.0 °C | 410 MPa Show Material materials with Tensile strength of 410 MPa | ||
250.0 °C | 390 MPa Show Material materials with Tensile strength of 390 MPa | ||
300.0 °C | 385 MPa Show Material materials with Tensile strength of 385 MPa | ||
350.0 °C | 380 MPa Show Material materials with Tensile strength of 380 MPa | ||
Tensile strength, transverse | 20.0 °C | 470 - 670 MPa Show Material materials with Tensile strength, transverse of 470 - 670 MPa | |
Yield strength Rp0.2 | 50.0 °C | 181 MPa Show Material materials with Yield strength Rp0.2 of 181 MPa | |
100.0 °C | 150 MPa Show Material materials with Yield strength Rp0.2 of 150 MPa | ||
150.0 °C | 140 MPa Show Material materials with Yield strength Rp0.2 of 140 MPa | ||
200.0 °C | 130 MPa Show Material materials with Yield strength Rp0.2 of 130 MPa | ||
250.0 °C | 120 MPa Show Material materials with Yield strength Rp0.2 of 120 MPa | ||
300.0 °C | 115 MPa Show Material materials with Yield strength Rp0.2 of 115 MPa | ||
350.0 °C | 110 MPa Show Material materials with Yield strength Rp0.2 of 110 MPa | ||
400.0 °C | 105 MPa Show Material materials with Yield strength Rp0.2 of 105 MPa | ||
Yield strength Rp0.2, transverse | 20.0 °C | 200 MPa Show Material materials with Yield strength Rp0.2, transverse of 200 MPa | |
Yield strength Rp1.0 | 50.0 °C | 217 MPa Show Material materials with Yield strength Rp1.0 of 217 MPa | |
100.0 °C | 180 MPa Show Material materials with Yield strength Rp1.0 of 180 MPa | ||
150.0 °C | 170 MPa Show Material materials with Yield strength Rp1.0 of 170 MPa | ||
200.0 °C | 160 MPa Show Material materials with Yield strength Rp1.0 of 160 MPa | ||
250.0 °C | 150 MPa Show Material materials with Yield strength Rp1.0 of 150 MPa | ||
300.0 °C | 140 MPa Show Material materials with Yield strength Rp1.0 of 140 MPa | ||
350.0 °C | 135 MPa Show Material materials with Yield strength Rp1.0 of 135 MPa | ||
400.0 °C | 130 MPa Show Material materials with Yield strength Rp1.0 of 130 MPa | ||
Yield strength Rp1.0, transverse | 20.0 °C | 240 MPa Show Material materials with Yield strength Rp1.0, transverse of 240 MPa |
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of thermal expansion | -100.0 °C | 1.49E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.49E-5 1/K | |
20.0 °C | 1.61E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.61E-5 1/K | ||
100.0 °C | 1.58E-5 - 1.67E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.58E-5 - 1.67E-5 1/K | ||
200.0 °C | 1.61E-5 - 1.72E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.61E-5 - 1.72E-5 1/K | ||
300.0 °C | 1.65E-5 - 1.77E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.65E-5 - 1.77E-5 1/K | ||
400.0 °C | 1.69E-5 - 1.81E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.69E-5 - 1.81E-5 1/K | ||
500.0 °C | 1.73E-5 - 1.84E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.73E-5 - 1.84E-5 1/K | ||
600.0 °C | 1.88E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.88E-5 1/K | ||
700.0 °C | 1.91E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.91E-5 1/K | ||
800.0 °C | 1.94E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.94E-5 1/K | ||
900.0 °C | 1.97E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.97E-5 1/K | ||
1000.0 °C | 2E-5 1/K Show Material materials with Coefficient of thermal expansion of 2E-5 1/K | ||
Melting point | 1230 - 1480 °C Show Material materials with Melting point of 1230 - 1480 °C | Typical for Austenitic Stainless Steel | |
Specific heat capacity | -100.0 °C | 440 J/(kg·K) Show Material materials with Specific heat capacity of 440 J/(kg·K) | |
20.0 °C | 450 - 472 J/(kg·K) Show Material materials with Specific heat capacity of 450 - 472 J/(kg·K) | ||
100.0 °C | 487 J/(kg·K) Show Material materials with Specific heat capacity of 487 J/(kg·K) | ||
200.0 °C | 503 J/(kg·K) Show Material materials with Specific heat capacity of 503 J/(kg·K) | ||
300.0 °C | 512 J/(kg·K) Show Material materials with Specific heat capacity of 512 J/(kg·K) | ||
400.0 °C | 520 J/(kg·K) Show Material materials with Specific heat capacity of 520 J/(kg·K) | ||
500.0 °C | 530 J/(kg·K) Show Material materials with Specific heat capacity of 530 J/(kg·K) | ||
600.0 °C | 541 J/(kg·K) Show Material materials with Specific heat capacity of 541 J/(kg·K) | ||
700.0 °C | 551 J/(kg·K) Show Material materials with Specific heat capacity of 551 J/(kg·K) | ||
800.0 °C | 559 J/(kg·K) Show Material materials with Specific heat capacity of 559 J/(kg·K) | ||
900.0 °C | 565 J/(kg·K) Show Material materials with Specific heat capacity of 565 J/(kg·K) | ||
1000.0 °C | 571 J/(kg·K) Show Material materials with Specific heat capacity of 571 J/(kg·K) | ||
Thermal conductivity | 20.0 °C | 11.9 - 14 W/(m·K) Show Material materials with Thermal conductivity of 11.9 - 14 W/(m·K) | |
100.0 °C | 13.3 W/(m·K) Show Material materials with Thermal conductivity of 13.3 W/(m·K) | ||
200.0 °C | 15.1 W/(m·K) Show Material materials with Thermal conductivity of 15.1 W/(m·K) | ||
300.0 °C | 16.7 W/(m·K) Show Material materials with Thermal conductivity of 16.7 W/(m·K) | ||
400.0 °C | 18.3 W/(m·K) Show Material materials with Thermal conductivity of 18.3 W/(m·K) | ||
500.0 °C | 19.8 W/(m·K) Show Material materials with Thermal conductivity of 19.8 W/(m·K) | ||
600.0 °C | 21.3 W/(m·K) Show Material materials with Thermal conductivity of 21.3 W/(m·K) | ||
700.0 °C | 22.8 W/(m·K) Show Material materials with Thermal conductivity of 22.8 W/(m·K) | ||
800.0 °C | 24.3 W/(m·K) Show Material materials with Thermal conductivity of 24.3 W/(m·K) | ||
900.0 °C | 25.7 W/(m·K) Show Material materials with Thermal conductivity of 25.7 W/(m·K) | ||
1000.0 °C | 27.1 W/(m·K) Show Material materials with Thermal conductivity of 27.1 W/(m·K) | ||
Thermal diffusivity | 20.0 °C | 3.3 mm²/s Show Material materials with Thermal diffusivity of 3.3 mm²/s | |
100.0 °C | 3.4 mm²/s Show Material materials with Thermal diffusivity of 3.4 mm²/s | ||
200.0 °C | 3.7 mm²/s Show Material materials with Thermal diffusivity of 3.7 mm²/s | ||
300.0 °C | 4.1 mm²/s Show Material materials with Thermal diffusivity of 4.1 mm²/s | ||
400.0 °C | 4.3 mm²/s Show Material materials with Thermal diffusivity of 4.3 mm²/s | ||
500.0 °C | 4.5 mm²/s Show Material materials with Thermal diffusivity of 4.5 mm²/s | ||
600.0 °C | 4.7 mm²/s Show Material materials with Thermal diffusivity of 4.7 mm²/s | ||
700.0 °C | 5 mm²/s Show Material materials with Thermal diffusivity of 5 mm²/s | ||
800.0 °C | 5.4 mm²/s Show Material materials with Thermal diffusivity of 5.4 mm²/s | ||
900.0 °C | 5.7 mm²/s Show Material materials with Thermal diffusivity of 5.7 mm²/s | ||
1000.0 °C | 5.8 mm²/s Show Material materials with Thermal diffusivity of 5.8 mm²/s | ||
Electrical
Property | Temperature | Value |
---|---|---|
Electrical resistivity | 20.0 °C | 8.5E-7 - 9.59E-7 Ω·m Show Material materials with Electrical resistivity of 8.5E-7 - 9.59E-7 Ω·m |
100.0 °C | 1.01E-6 Ω·m Show Material materials with Electrical resistivity of 1.01E-6 Ω·m | |
200.0 °C | 1.05E-6 Ω·m Show Material materials with Electrical resistivity of 1.05E-6 Ω·m | |
300.0 °C | 1.1E-6 Ω·m Show Material materials with Electrical resistivity of 1.1E-6 Ω·m | |
400.0 °C | 1.13E-6 Ω·m Show Material materials with Electrical resistivity of 1.13E-6 Ω·m | |
500.0 °C | 1.17E-6 Ω·m Show Material materials with Electrical resistivity of 1.17E-6 Ω·m | |
600.0 °C | 1.19E-6 Ω·m Show Material materials with Electrical resistivity of 1.19E-6 Ω·m | |
700.0 °C | 1.22E-6 Ω·m Show Material materials with Electrical resistivity of 1.22E-6 Ω·m | |
800.0 °C | 1.24E-6 Ω·m Show Material materials with Electrical resistivity of 1.24E-6 Ω·m | |
900.0 °C | 1.26E-6 Ω·m Show Material materials with Electrical resistivity of 1.26E-6 Ω·m | |
1000.0 °C | 1.28E-6 Ω·m Show Material materials with Electrical resistivity of 1.28E-6 Ω·m | |
Chemical properties
Property | Value |
---|---|
Carbon | 0.02 % Show Material materials with Carbon of 0.02 % |
Chromium | 24 - 26 % Show Material materials with Chromium of 24 - 26 % |
Manganese | 2 % Show Material materials with Manganese of 2 % |
Molybdenum | 0.2 % Show Material materials with Molybdenum of 0.2 % |
Nickel | 20 - 22 % Show Material materials with Nickel of 20 - 22 % |
Nitrogen | 0.1 - 0.11 % Show Material materials with Nitrogen of 0.1 - 0.11 % |
Phosphorus | 0.03 % Show Material materials with Phosphorus of 0.03 % |
Silicon | 0.25 % Show Material materials with Silicon of 0.25 % |
Sulfur | 0.01 % Show Material materials with Sulfur of 0.01 % |
Do you have a technical question or need more information about this material?
Post it as a comment below and receive answers from engineers and other community members.