EN 10028-7 Grade X6CrNiMoNb17-12-2 solution annealed (+AT)

Want to keep this datasheet? Save it now in your required format

Description

The austenitic steel X6CrNiMoNb17-12-2 is comparable to 1.4571 regarding corrosion properties. Increased corrosion resistance to nonoxidizing acids and halogenated media. The material is resistant to intercrystalline corrosion even in sensitized condition. The steel is not mirror-polishable. It is permitted for pressure vessel engineering up to 300 °C. Up to 550 °C if there are no media causing intercrystalline attack. Application: in chemical apparatus engineering, in textile-, sulfite-, cellulose, fatty acid-, rubber and coloring industry

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

7.96 - 8 g/cm³

Show Material materials with Density of 7.96 - 8 g/cm³

Mechanical

PropertyTemperatureValue

Elastic modulus

-100.0 °C

206 GPa

Show Material materials with Elastic modulus of 206 GPa

20.0 °C

196 - 200 GPa

Show Material materials with Elastic modulus of 196 - 200 GPa

100.0 °C

190 - 194 GPa

Show Material materials with Elastic modulus of 190 - 194 GPa

200.0 °C

182 - 186 GPa

Show Material materials with Elastic modulus of 182 - 186 GPa

300.0 °C

174 - 179 GPa

Show Material materials with Elastic modulus of 174 - 179 GPa

400.0 °C

166 - 172 GPa

Show Material materials with Elastic modulus of 166 - 172 GPa

500.0 °C

158 - 165 GPa

Show Material materials with Elastic modulus of 158 - 165 GPa

600.0 °C

150 GPa

Show Material materials with Elastic modulus of 150 GPa

700.0 °C

142 GPa

Show Material materials with Elastic modulus of 142 GPa

800.0 °C

134 GPa

Show Material materials with Elastic modulus of 134 GPa

900.0 °C

127 GPa

Show Material materials with Elastic modulus of 127 GPa

1000.0 °C

120 GPa

Show Material materials with Elastic modulus of 120 GPa

Elongation A80, transverse

20.0 °C

40 %

Show Material materials with Elongation A80, transverse of 40 %

Elongation, transverse

20.0 °C

40 %

Show Material materials with Elongation, transverse of 40 %

Poisson's ratio

20.0 °C

0.28 [-]

Show Material materials with Poisson's ratio of 0.28 [-]

Shear modulus

20.0 °C

77.01 GPa

Show Material materials with Shear modulus of 77.01 GPa

Tensile strength

20.0 °C

520 - 720 MPa

Show Material materials with Tensile strength of 520 - 720 MPa

50.0 °C

490 MPa

Show Material materials with Tensile strength of 490 MPa

100.0 °C

440 MPa

Show Material materials with Tensile strength of 440 MPa

150.0 °C

410 MPa

Show Material materials with Tensile strength of 410 MPa

200.0 °C

390 MPa

Show Material materials with Tensile strength of 390 MPa

250.0 °C

385 MPa

Show Material materials with Tensile strength of 385 MPa

300.0 °C

375 MPa

Show Material materials with Tensile strength of 375 MPa

350.0 °C

375 MPa

Show Material materials with Tensile strength of 375 MPa

400.0 °C

375 MPa

Show Material materials with Tensile strength of 375 MPa

450.0 °C

370 MPa

Show Material materials with Tensile strength of 370 MPa

500.0 °C

360 MPa

Show Material materials with Tensile strength of 360 MPa

550.0 °C

330 MPa

Show Material materials with Tensile strength of 330 MPa

Unlock all property charts

Tensile strength, transverse

20.0 °C

520 - 720 MPa

Show Material materials with Tensile strength, transverse of 520 - 720 MPa

Yield strength Rp0.2

50.0 °C

207 MPa

Show Material materials with Yield strength Rp0.2 of 207 MPa

100.0 °C

185 MPa

Show Material materials with Yield strength Rp0.2 of 185 MPa

150.0 °C

177 MPa

Show Material materials with Yield strength Rp0.2 of 177 MPa

200.0 °C

167 MPa

Show Material materials with Yield strength Rp0.2 of 167 MPa

250.0 °C

157 MPa

Show Material materials with Yield strength Rp0.2 of 157 MPa

300.0 °C

145 MPa

Show Material materials with Yield strength Rp0.2 of 145 MPa

350.0 °C

140 MPa

Show Material materials with Yield strength Rp0.2 of 140 MPa

400.0 °C

135 MPa

Show Material materials with Yield strength Rp0.2 of 135 MPa

450.0 °C

131 MPa

Show Material materials with Yield strength Rp0.2 of 131 MPa

500.0 °C

129 MPa

Show Material materials with Yield strength Rp0.2 of 129 MPa

550.0 °C

127 MPa

Show Material materials with Yield strength Rp0.2 of 127 MPa

Unlock all property charts

Yield strength Rp0.2, transverse

20.0 °C

220 MPa

Show Material materials with Yield strength Rp0.2, transverse of 220 MPa

Yield strength Rp1.0

50.0 °C

244 MPa

Show Material materials with Yield strength Rp1.0 of 244 MPa

100.0 °C

218 MPa

Show Material materials with Yield strength Rp1.0 of 218 MPa

150.0 °C

206 MPa

Show Material materials with Yield strength Rp1.0 of 206 MPa

200.0 °C

196 MPa

Show Material materials with Yield strength Rp1.0 of 196 MPa

250.0 °C

186 MPa

Show Material materials with Yield strength Rp1.0 of 186 MPa

300.0 °C

175 MPa

Show Material materials with Yield strength Rp1.0 of 175 MPa

350.0 °C

169 MPa

Show Material materials with Yield strength Rp1.0 of 169 MPa

400.0 °C

164 MPa

Show Material materials with Yield strength Rp1.0 of 164 MPa

450.0 °C

160 MPa

Show Material materials with Yield strength Rp1.0 of 160 MPa

500.0 °C

158 MPa

Show Material materials with Yield strength Rp1.0 of 158 MPa

550.0 °C

157 MPa

Show Material materials with Yield strength Rp1.0 of 157 MPa

Unlock all property charts

Yield strength Rp1.0, transverse

20.0 °C

260 MPa

Show Material materials with Yield strength Rp1.0, transverse of 260 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

-100.0 °C

1.49E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.49E-5 1/K

20.0 °C

1.61E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.61E-5 1/K

100.0 °C

1.65E-5 - 1.67E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.65E-5 - 1.67E-5 1/K

200.0 °C

1.72E-5 - 1.75E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.72E-5 - 1.75E-5 1/K

300.0 °C

1.77E-5 - 1.8E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.77E-5 - 1.8E-5 1/K

400.0 °C

1.81E-5 - 1.85E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.81E-5 - 1.85E-5 1/K

500.0 °C

1.84E-5 - 1.9E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.84E-5 - 1.9E-5 1/K

600.0 °C

1.88E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.88E-5 1/K

700.0 °C

1.91E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.91E-5 1/K

800.0 °C

1.94E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.94E-5 1/K

900.0 °C

1.97E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.97E-5 1/K

1000.0 °C

2E-5 1/K

Show Material materials with Coefficient of thermal expansion of 2E-5 1/K

Unlock all property charts

Max service temperature, long

0 - 550 °C

Show Material materials with Max service temperature, long of 0 - 550 °C

Melting point

1230 - 1480 °C

Show Material materials with Melting point of 1230 - 1480 °C

Typical for Austenitic Stainless Steel

Specific heat capacity

-100.0 °C

440 J/(kg·K)

Show Material materials with Specific heat capacity of 440 J/(kg·K)

20.0 °C

472 - 500 J/(kg·K)

Show Material materials with Specific heat capacity of 472 - 500 J/(kg·K)

100.0 °C

487 J/(kg·K)

Show Material materials with Specific heat capacity of 487 J/(kg·K)

200.0 °C

503 J/(kg·K)

Show Material materials with Specific heat capacity of 503 J/(kg·K)

300.0 °C

512 J/(kg·K)

Show Material materials with Specific heat capacity of 512 J/(kg·K)

400.0 °C

520 J/(kg·K)

Show Material materials with Specific heat capacity of 520 J/(kg·K)

500.0 °C

530 J/(kg·K)

Show Material materials with Specific heat capacity of 530 J/(kg·K)

600.0 °C

541 J/(kg·K)

Show Material materials with Specific heat capacity of 541 J/(kg·K)

700.0 °C

551 J/(kg·K)

Show Material materials with Specific heat capacity of 551 J/(kg·K)

800.0 °C

559 J/(kg·K)

Show Material materials with Specific heat capacity of 559 J/(kg·K)

900.0 °C

565 J/(kg·K)

Show Material materials with Specific heat capacity of 565 J/(kg·K)

1000.0 °C

571 J/(kg·K)

Show Material materials with Specific heat capacity of 571 J/(kg·K)

Unlock all property charts

Thermal conductivity

20.0 °C

13.3 - 15 W/(m·K)

Show Material materials with Thermal conductivity of 13.3 - 15 W/(m·K)

100.0 °C

14.9 W/(m·K)

Show Material materials with Thermal conductivity of 14.9 W/(m·K)

200.0 °C

16.5 W/(m·K)

Show Material materials with Thermal conductivity of 16.5 W/(m·K)

300.0 °C

18.1 W/(m·K)

Show Material materials with Thermal conductivity of 18.1 W/(m·K)

400.0 °C

19.5 W/(m·K)

Show Material materials with Thermal conductivity of 19.5 W/(m·K)

500.0 °C

21 W/(m·K)

Show Material materials with Thermal conductivity of 21 W/(m·K)

600.0 °C

22.4 W/(m·K)

Show Material materials with Thermal conductivity of 22.4 W/(m·K)

700.0 °C

23.8 W/(m·K)

Show Material materials with Thermal conductivity of 23.8 W/(m·K)

800.0 °C

25.2 W/(m·K)

Show Material materials with Thermal conductivity of 25.2 W/(m·K)

Unlock all property charts

Thermal diffusivity

20.0 °C

3.5 mm²/s

Show Material materials with Thermal diffusivity of 3.5 mm²/s

100.0 °C

3.8 mm²/s

Show Material materials with Thermal diffusivity of 3.8 mm²/s

200.0 °C

4 mm²/s

Show Material materials with Thermal diffusivity of 4 mm²/s

300.0 °C

4.3 mm²/s

Show Material materials with Thermal diffusivity of 4.3 mm²/s

400.0 °C

4.5 mm²/s

Show Material materials with Thermal diffusivity of 4.5 mm²/s

500.0 °C

4.7 mm²/s

Show Material materials with Thermal diffusivity of 4.7 mm²/s

600.0 °C

4.8 mm²/s

Show Material materials with Thermal diffusivity of 4.8 mm²/s

700.0 °C

5.1 mm²/s

Show Material materials with Thermal diffusivity of 5.1 mm²/s

800.0 °C

5.4 mm²/s

Show Material materials with Thermal diffusivity of 5.4 mm²/s

Unlock all property charts

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

7.5E-7 - 7.91E-7 Ω·m

Show Material materials with Electrical resistivity of 7.5E-7 - 7.91E-7 Ω·m

100.0 °C

8.45E-7 Ω·m

Show Material materials with Electrical resistivity of 8.45E-7 Ω·m

200.0 °C

9.19E-7 Ω·m

Show Material materials with Electrical resistivity of 9.19E-7 Ω·m

300.0 °C

9.77E-7 Ω·m

Show Material materials with Electrical resistivity of 9.77E-7 Ω·m

400.0 °C

1.03E-6 Ω·m

Show Material materials with Electrical resistivity of 1.03E-6 Ω·m

500.0 °C

1.08E-6 Ω·m

Show Material materials with Electrical resistivity of 1.08E-6 Ω·m

600.0 °C

1.12E-6 Ω·m

Show Material materials with Electrical resistivity of 1.12E-6 Ω·m

700.0 °C

1.15E-6 Ω·m

Show Material materials with Electrical resistivity of 1.15E-6 Ω·m

800.0 °C

1.18E-6 Ω·m

Show Material materials with Electrical resistivity of 1.18E-6 Ω·m

Unlock all property charts

Chemical properties

PropertyValue

Carbon

0.08 %

Show Material materials with Carbon of 0.08 %

Chromium

16.5 - 18.5 %

Show Material materials with Chromium of 16.5 - 18.5 %

Manganese

2 %

Show Material materials with Manganese of 2 %

Molybdenum

2 - 2.5 %

Show Material materials with Molybdenum of 2 - 2.5 %

Nickel

10.5 - 13.5 %

Show Material materials with Nickel of 10.5 - 13.5 %

Niobium

1 %

Show Material materials with Niobium of 1 %

Phosphorus

0.05 %

Show Material materials with Phosphorus of 0.05 %

Silicon

1 %

Show Material materials with Silicon of 1 %

Sulfur

0.015 %

Show Material materials with Sulfur of 0.015 %