The austenitic steel X2CrNiMo18-15-4 shows very high resistance to unoxidizing and halogenated media due to its high Mo-content (more than 3%), furthermore resistance to intercrystalline corrosion even in sensitized condition. It is usable for mirror-polishing and is cold formable. The steel is permitted for pressure vessel construction. Application: in chemical apparatus engineering especially in cellulose industry, in textile and rayon industry, in tankship construction and for transport containers

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

8 - 8.01 g/cm³

Show Material materials with Density of 8 - 8.01 g/cm³

Mechanical

PropertyTemperatureValue

Elastic modulus

-100.0 °C

206 GPa

Show Material materials with Elastic modulus of 206 GPa

20.0 °C

196 - 200 GPa

Show Material materials with Elastic modulus of 196 - 200 GPa

100.0 °C

190 - 194 GPa

Show Material materials with Elastic modulus of 190 - 194 GPa

200.0 °C

182 - 186 GPa

Show Material materials with Elastic modulus of 182 - 186 GPa

300.0 °C

174 - 179 GPa

Show Material materials with Elastic modulus of 174 - 179 GPa

400.0 °C

166 - 172 GPa

Show Material materials with Elastic modulus of 166 - 172 GPa

500.0 °C

158 - 165 GPa

Show Material materials with Elastic modulus of 158 - 165 GPa

600.0 °C

150 GPa

Show Material materials with Elastic modulus of 150 GPa

700.0 °C

142 GPa

Show Material materials with Elastic modulus of 142 GPa

800.0 °C

134 GPa

Show Material materials with Elastic modulus of 134 GPa

Elongation A80, transverse

20.0 °C

35 - 40 %

Show Material materials with Elongation A80, transverse of 35 - 40 %

Elongation, transverse

20.0 °C

35 - 40 %

Show Material materials with Elongation, transverse of 35 - 40 %

Poisson's ratio

20.0 °C

0.28 [-]

Show Material materials with Poisson's ratio of 0.28 [-]

Shear modulus

20.0 °C

77.3 GPa

Show Material materials with Shear modulus of 77.3 GPa

Tensile strength

20.0 °C

520 - 720 MPa

Show Material materials with Tensile strength of 520 - 720 MPa

50.0 °C

486 MPa

Show Material materials with Tensile strength of 486 MPa

100.0 °C

430 MPa

Show Material materials with Tensile strength of 430 MPa

150.0 °C

410 MPa

Show Material materials with Tensile strength of 410 MPa

200.0 °C

390 MPa

Show Material materials with Tensile strength of 390 MPa

250.0 °C

385 MPa

Show Material materials with Tensile strength of 385 MPa

300.0 °C

380 MPa

Show Material materials with Tensile strength of 380 MPa

350.0 °C

380 MPa

Show Material materials with Tensile strength of 380 MPa

Unlock all property charts

Tensile strength, transverse

20.0 °C

520 - 720 MPa

Show Material materials with Tensile strength, transverse of 520 - 720 MPa

Yield strength Rp0.2

50.0 °C

202 MPa

Show Material materials with Yield strength Rp0.2 of 202 MPa

100.0 °C

172 MPa

Show Material materials with Yield strength Rp0.2 of 172 MPa

150.0 °C

157 MPa

Show Material materials with Yield strength Rp0.2 of 157 MPa

200.0 °C

147 MPa

Show Material materials with Yield strength Rp0.2 of 147 MPa

250.0 °C

137 MPa

Show Material materials with Yield strength Rp0.2 of 137 MPa

300.0 °C

127 MPa

Show Material materials with Yield strength Rp0.2 of 127 MPa

350.0 °C

120 MPa

Show Material materials with Yield strength Rp0.2 of 120 MPa

400.0 °C

115 MPa

Show Material materials with Yield strength Rp0.2 of 115 MPa

450.0 °C

112 MPa

Show Material materials with Yield strength Rp0.2 of 112 MPa

500.0 °C

110 MPa

Show Material materials with Yield strength Rp0.2 of 110 MPa

550.0 °C

108 MPa

Show Material materials with Yield strength Rp0.2 of 108 MPa

Unlock all property charts

Yield strength Rp0.2, transverse

20.0 °C

220 - 240 MPa

Show Material materials with Yield strength Rp0.2, transverse of 220 - 240 MPa

Yield strength Rp1.0

50.0 °C

240 MPa

Show Material materials with Yield strength Rp1.0 of 240 MPa

100.0 °C

206 MPa

Show Material materials with Yield strength Rp1.0 of 206 MPa

150.0 °C

188 MPa

Show Material materials with Yield strength Rp1.0 of 188 MPa

200.0 °C

177 MPa

Show Material materials with Yield strength Rp1.0 of 177 MPa

250.0 °C

167 MPa

Show Material materials with Yield strength Rp1.0 of 167 MPa

300.0 °C

156 MPa

Show Material materials with Yield strength Rp1.0 of 156 MPa

350.0 °C

148 MPa

Show Material materials with Yield strength Rp1.0 of 148 MPa

400.0 °C

144 MPa

Show Material materials with Yield strength Rp1.0 of 144 MPa

450.0 °C

140 MPa

Show Material materials with Yield strength Rp1.0 of 140 MPa

500.0 °C

138 MPa

Show Material materials with Yield strength Rp1.0 of 138 MPa

550.0 °C

136 MPa

Show Material materials with Yield strength Rp1.0 of 136 MPa

Unlock all property charts

Yield strength Rp1.0, transverse

20.0 °C

260 - 270 MPa

Show Material materials with Yield strength Rp1.0, transverse of 260 - 270 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

-100.0 °C

1.49E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.49E-5 1/K

20.0 °C

1.61E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.61E-5 1/K

100.0 °C

1.6E-5 - 1.67E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.6E-5 - 1.67E-5 1/K

200.0 °C

1.65E-5 - 1.72E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.65E-5 - 1.72E-5 1/K

300.0 °C

1.7E-5 - 1.77E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.7E-5 - 1.77E-5 1/K

400.0 °C

1.75E-5 - 1.81E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.75E-5 - 1.81E-5 1/K

500.0 °C

1.8E-5 - 1.84E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.8E-5 - 1.84E-5 1/K

600.0 °C

1.88E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.88E-5 1/K

700.0 °C

1.91E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.91E-5 1/K

800.0 °C

1.94E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.94E-5 1/K

900.0 °C

1.97E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.97E-5 1/K

1000.0 °C

2E-5 1/K

Show Material materials with Coefficient of thermal expansion of 2E-5 1/K

Unlock all property charts

Melting point

1230 - 1480 °C

Show Material materials with Melting point of 1230 - 1480 °C

Typical for Austenitic Stainless Steel

Specific heat capacity

-100.0 °C

440 J/(kg·K)

Show Material materials with Specific heat capacity of 440 J/(kg·K)

20.0 °C

472 - 500 J/(kg·K)

Show Material materials with Specific heat capacity of 472 - 500 J/(kg·K)

100.0 °C

487 J/(kg·K)

Show Material materials with Specific heat capacity of 487 J/(kg·K)

200.0 °C

503 J/(kg·K)

Show Material materials with Specific heat capacity of 503 J/(kg·K)

300.0 °C

512 J/(kg·K)

Show Material materials with Specific heat capacity of 512 J/(kg·K)

400.0 °C

520 J/(kg·K)

Show Material materials with Specific heat capacity of 520 J/(kg·K)

500.0 °C

530 J/(kg·K)

Show Material materials with Specific heat capacity of 530 J/(kg·K)

600.0 °C

541 J/(kg·K)

Show Material materials with Specific heat capacity of 541 J/(kg·K)

700.0 °C

551 J/(kg·K)

Show Material materials with Specific heat capacity of 551 J/(kg·K)

800.0 °C

559 J/(kg·K)

Show Material materials with Specific heat capacity of 559 J/(kg·K)

900.0 °C

565 J/(kg·K)

Show Material materials with Specific heat capacity of 565 J/(kg·K)

1000.0 °C

571 J/(kg·K)

Show Material materials with Specific heat capacity of 571 J/(kg·K)

Unlock all property charts

Thermal conductivity

20.0 °C

13.5 - 14 W/(m·K)

Show Material materials with Thermal conductivity of 13.5 - 14 W/(m·K)

100.0 °C

14.9 W/(m·K)

Show Material materials with Thermal conductivity of 14.9 W/(m·K)

200.0 °C

16.7 W/(m·K)

Show Material materials with Thermal conductivity of 16.7 W/(m·K)

300.0 °C

18.3 W/(m·K)

Show Material materials with Thermal conductivity of 18.3 W/(m·K)

400.0 °C

19.8 W/(m·K)

Show Material materials with Thermal conductivity of 19.8 W/(m·K)

500.0 °C

21.3 W/(m·K)

Show Material materials with Thermal conductivity of 21.3 W/(m·K)

600.0 °C

22.7 W/(m·K)

Show Material materials with Thermal conductivity of 22.7 W/(m·K)

700.0 °C

24.2 W/(m·K)

Show Material materials with Thermal conductivity of 24.2 W/(m·K)

800.0 °C

25.6 W/(m·K)

Show Material materials with Thermal conductivity of 25.6 W/(m·K)

Unlock all property charts

Thermal diffusivity

20.0 °C

3.6 mm²/s

Show Material materials with Thermal diffusivity of 3.6 mm²/s

100.0 °C

3.7 mm²/s

Show Material materials with Thermal diffusivity of 3.7 mm²/s

200.0 °C

4 mm²/s

Show Material materials with Thermal diffusivity of 4 mm²/s

300.0 °C

4.4 mm²/s

Show Material materials with Thermal diffusivity of 4.4 mm²/s

400.0 °C

4.6 mm²/s

Show Material materials with Thermal diffusivity of 4.6 mm²/s

500.0 °C

4.7 mm²/s

Show Material materials with Thermal diffusivity of 4.7 mm²/s

600.0 °C

4.9 mm²/s

Show Material materials with Thermal diffusivity of 4.9 mm²/s

700.0 °C

5.2 mm²/s

Show Material materials with Thermal diffusivity of 5.2 mm²/s

800.0 °C

5.5 mm²/s

Show Material materials with Thermal diffusivity of 5.5 mm²/s

Unlock all property charts

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

7.75E-7 - 8.5E-7 Ω·m

Show Material materials with Electrical resistivity of 7.75E-7 - 8.5E-7 Ω·m

100.0 °C

8.42E-7 Ω·m

Show Material materials with Electrical resistivity of 8.42E-7 Ω·m

200.0 °C

9.04E-7 Ω·m

Show Material materials with Electrical resistivity of 9.04E-7 Ω·m

300.0 °C

9.62E-7 Ω·m

Show Material materials with Electrical resistivity of 9.62E-7 Ω·m

400.0 °C

1.01E-6 Ω·m

Show Material materials with Electrical resistivity of 1.01E-6 Ω·m

500.0 °C

1.06E-6 Ω·m

Show Material materials with Electrical resistivity of 1.06E-6 Ω·m

600.0 °C

1.1E-6 Ω·m

Show Material materials with Electrical resistivity of 1.1E-6 Ω·m

700.0 °C

1.13E-6 Ω·m

Show Material materials with Electrical resistivity of 1.13E-6 Ω·m

800.0 °C

1.16E-6 Ω·m

Show Material materials with Electrical resistivity of 1.16E-6 Ω·m

Unlock all property charts

Chemical properties

PropertyValue

Carbon

0.03 %

Show Material materials with Carbon of 0.03 %

Chromium

17.5 - 19.5 %

Show Material materials with Chromium of 17.5 - 19.5 %

Manganese

2 %

Show Material materials with Manganese of 2 %

Molybdenum

3 - 4 %

Show Material materials with Molybdenum of 3 - 4 %

Nickel

13 - 16 %

Show Material materials with Nickel of 13 - 16 %

Nitrogen

0.1 - 0.11 %

Show Material materials with Nitrogen of 0.1 - 0.11 %

Phosphorus

0.05 %

Show Material materials with Phosphorus of 0.05 %

Silicon

1 %

Show Material materials with Silicon of 1 %

Sulfur