General
Property | Temperature | Value |
---|---|---|
Density | 20.0 °C | 8.1 g/cm³ Show Material materials with Density of 8.1 g/cm³ |
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elastic modulus | 20.0 °C | 195 GPa Show Material materials with Elastic modulus of 195 GPa | |
100.0 °C | 190 GPa Show Material materials with Elastic modulus of 190 GPa | ||
200.0 °C | 182 GPa Show Material materials with Elastic modulus of 182 GPa | ||
300.0 °C | 174 GPa Show Material materials with Elastic modulus of 174 GPa | ||
400.0 °C | 166 GPa Show Material materials with Elastic modulus of 166 GPa | ||
500.0 °C | 158 GPa Show Material materials with Elastic modulus of 158 GPa | ||
Elongation A80, transverse | 20.0 °C | 40 % Show Material materials with Elongation A80, transverse of 40 % | |
Elongation, transverse | 20.0 °C | 40 % Show Material materials with Elongation, transverse of 40 % | |
Poisson's ratio | 23.0 °C | 0.3 [-] Show Material materials with Poisson's ratio of 0.3 [-] | Typical for Austenitic Stainless Steel |
Shear modulus | 23.0 °C | 77 GPa Show Material materials with Shear modulus of 77 GPa | Typical for Austenitic Stainless Steel |
Tensile strength | 20.0 °C | 600 - 800 MPa Show Material materials with Tensile strength of 600 - 800 MPa | |
50.0 °C | 581 MPa Show Material materials with Tensile strength of 581 MPa | ||
100.0 °C | 550 MPa Show Material materials with Tensile strength of 550 MPa | ||
150.0 °C | 535 MPa Show Material materials with Tensile strength of 535 MPa | ||
200.0 °C | 520 MPa Show Material materials with Tensile strength of 520 MPa | ||
250.0 °C | 500 MPa Show Material materials with Tensile strength of 500 MPa | ||
300.0 °C | 480 MPa Show Material materials with Tensile strength of 480 MPa | ||
350.0 °C | 475 MPa Show Material materials with Tensile strength of 475 MPa | ||
Tensile strength, transverse | 20.0 °C | 600 - 800 MPa Show Material materials with Tensile strength, transverse of 600 - 800 MPa | |
Yield strength Rp0.2 | 50.0 °C | 271 MPa Show Material materials with Yield strength Rp0.2 of 271 MPa | |
100.0 °C | 240 MPa Show Material materials with Yield strength Rp0.2 of 240 MPa | ||
150.0 °C | 220 MPa Show Material materials with Yield strength Rp0.2 of 220 MPa | ||
200.0 °C | 200 MPa Show Material materials with Yield strength Rp0.2 of 200 MPa | ||
250.0 °C | 190 MPa Show Material materials with Yield strength Rp0.2 of 190 MPa | ||
300.0 °C | 180 MPa Show Material materials with Yield strength Rp0.2 of 180 MPa | ||
350.0 °C | 175 MPa Show Material materials with Yield strength Rp0.2 of 175 MPa | ||
400.0 °C | 170 MPa Show Material materials with Yield strength Rp0.2 of 170 MPa | ||
Yield strength Rp0.2, transverse | 20.0 °C | 290 MPa Show Material materials with Yield strength Rp0.2, transverse of 290 MPa | |
Yield strength Rp1.0 | 50.0 °C | 307 MPa Show Material materials with Yield strength Rp1.0 of 307 MPa | |
100.0 °C | 270 MPa Show Material materials with Yield strength Rp1.0 of 270 MPa | ||
150.0 °C | 250 MPa Show Material materials with Yield strength Rp1.0 of 250 MPa | ||
200.0 °C | 230 MPa Show Material materials with Yield strength Rp1.0 of 230 MPa | ||
250.0 °C | 220 MPa Show Material materials with Yield strength Rp1.0 of 220 MPa | ||
300.0 °C | 210 MPa Show Material materials with Yield strength Rp1.0 of 210 MPa | ||
350.0 °C | 205 MPa Show Material materials with Yield strength Rp1.0 of 205 MPa | ||
400.0 °C | 200 MPa Show Material materials with Yield strength Rp1.0 of 200 MPa | ||
Yield strength Rp1.0, transverse | 20.0 °C | 330 MPa Show Material materials with Yield strength Rp1.0, transverse of 330 MPa |
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of thermal expansion | 100.0 °C | 1.5E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.5E-5 1/K | |
300.0 °C | 1.65E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.65E-5 1/K | ||
Melting point | 1230 - 1480 °C Show Material materials with Melting point of 1230 - 1480 °C | Typical for Austenitic Stainless Steel | |
Specific heat capacity | 20.0 °C | 500 J/(kg·K) Show Material materials with Specific heat capacity of 500 J/(kg·K) | |
Thermal conductivity | 20.0 °C | 14 W/(m·K) Show Material materials with Thermal conductivity of 14 W/(m·K) |
Electrical
Property | Temperature | Value |
---|---|---|
Electrical resistivity | 20.0 °C | 8.5E-7 Ω·m Show Material materials with Electrical resistivity of 8.5E-7 Ω·m |
Chemical properties
Property | Value |
---|---|
Carbon | 0.02 % Show Material materials with Carbon of 0.02 % |
Chromium | 24 - 26 % Show Material materials with Chromium of 24 - 26 % |
Copper | 1 - 2 % Show Material materials with Copper of 1 - 2 % |
Manganese | 2 % Show Material materials with Manganese of 2 % |
Molybdenum | 4.7 - 5.7 % Show Material materials with Molybdenum of 4.7 - 5.7 % |
Nickel | 24 - 27 % Show Material materials with Nickel of 24 - 27 % |
Nitrogen | 0.17 - 0.25 % Show Material materials with Nitrogen of 0.17 - 0.25 % |
Phosphorus | 0.03 % Show Material materials with Phosphorus of 0.03 % |
Silicon | 0.7 % Show Material materials with Silicon of 0.7 % |
Sulfur | 0.01 % Show Material materials with Sulfur of 0.01 % |