EN 10028-7 Grade X1NiCrMoCuN25-20-7 solution annealed (+AT)

View all suppliers (8)

Want to keep this datasheet? Save it now in your required format

Description

The austenitic steel X1NiCrMoCuN25-20-7 is the stronger Mo-alloyed type of the 1.4539. The steel shows a very high resistance to crevice corrosion, pitting corrosion as well as to stress corrosion caused by pitting corrosion. It has the highest pitting index with 46. The material is resistant to intercrystalline corrosion, even in welded condition. Application: in higher chloride-contaminated media, e.g. in appropriate sulphur and phosphorus acids, furthermore in offshore engineering

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

"Typical" values were obtained via a literature search. "Predicted" values were imputed via artificial intelligence technology. While we have placed significant efforts in ensuring data accuracy, "typical" and "predicted" data should be considered indicative and verified by appropriate material testing. Please do contact us if additional information on the the predicted data method is required.
All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

7.76 - 8.1 g/cm³

Show Material materials with Density of 7.76 - 8.1 g/cm³

Mechanical

PropertyTemperatureValueComment

Elastic modulus

-100.0 °C

206 GPa

Show Material materials with Elastic modulus of 206 GPa

20.0 °C

195 - 196 GPa

Show Material materials with Elastic modulus of 195 - 196 GPa

100.0 °C

190 GPa

Show Material materials with Elastic modulus of 190 GPa

200.0 °C

182 GPa

Show Material materials with Elastic modulus of 182 GPa

300.0 °C

174 GPa

Show Material materials with Elastic modulus of 174 GPa

400.0 °C

166 GPa

Show Material materials with Elastic modulus of 166 GPa

500.0 °C

158 GPa

Show Material materials with Elastic modulus of 158 GPa

600.0 °C

150 GPa

Show Material materials with Elastic modulus of 150 GPa

700.0 °C

142 GPa

Show Material materials with Elastic modulus of 142 GPa

800.0 °C

134 GPa

Show Material materials with Elastic modulus of 134 GPa

900.0 °C

127 GPa

Show Material materials with Elastic modulus of 127 GPa

1000.0 °C

120 GPa

Show Material materials with Elastic modulus of 120 GPa

Elongation A80, transverse

20.0 °C

40 %

Show Material materials with Elongation A80, transverse of 40 %

Elongation, transverse

20.0 °C

40 %

Show Material materials with Elongation, transverse of 40 %

Poisson's ratio

23.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

Typical for Austenitic Stainless Steel

Shear modulus

23.0 °C

77 GPa

Show Material materials with Shear modulus of 77 GPa

Typical for Austenitic Stainless Steel

Tensile strength

20.0 °C

650 - 850 MPa

Show Material materials with Tensile strength of 650 - 850 MPa

50.0 °C

612 MPa

Show Material materials with Tensile strength of 612 MPa

100.0 °C

550 MPa

Show Material materials with Tensile strength of 550 MPa

150.0 °C

535 MPa

Show Material materials with Tensile strength of 535 MPa

200.0 °C

520 MPa

Show Material materials with Tensile strength of 520 MPa

250.0 °C

500 MPa

Show Material materials with Tensile strength of 500 MPa

300.0 °C

480 MPa

Show Material materials with Tensile strength of 480 MPa

350.0 °C

475 MPa

Show Material materials with Tensile strength of 475 MPa

Unlock all property charts

Tensile strength, transverse

20.0 °C

650 - 850 MPa

Show Material materials with Tensile strength, transverse of 650 - 850 MPa

Yield strength Rp0.2

50.0 °C

274 MPa

Show Material materials with Yield strength Rp0.2 of 274 MPa

100.0 °C

230 MPa

Show Material materials with Yield strength Rp0.2 of 230 MPa

150.0 °C

210 MPa

Show Material materials with Yield strength Rp0.2 of 210 MPa

200.0 °C

190 MPa

Show Material materials with Yield strength Rp0.2 of 190 MPa

250.0 °C

180 MPa

Show Material materials with Yield strength Rp0.2 of 180 MPa

300.0 °C

170 MPa

Show Material materials with Yield strength Rp0.2 of 170 MPa

350.0 °C

165 MPa

Show Material materials with Yield strength Rp0.2 of 165 MPa

400.0 °C

160 MPa

Show Material materials with Yield strength Rp0.2 of 160 MPa

450.0 °C

130 MPa

Show Material materials with Yield strength Rp0.2 of 130 MPa

500.0 °C

120 MPa

Show Material materials with Yield strength Rp0.2 of 120 MPa

550.0 °C

105 MPa

Show Material materials with Yield strength Rp0.2 of 105 MPa

Unlock all property charts

Yield strength Rp0.2, transverse

20.0 °C

300 MPa

Show Material materials with Yield strength Rp0.2, transverse of 300 MPa

Yield strength Rp1.0

50.0 °C

314 MPa

Show Material materials with Yield strength Rp1.0 of 314 MPa

100.0 °C

270 MPa

Show Material materials with Yield strength Rp1.0 of 270 MPa

150.0 °C

245 MPa

Show Material materials with Yield strength Rp1.0 of 245 MPa

200.0 °C

225 MPa

Show Material materials with Yield strength Rp1.0 of 225 MPa

250.0 °C

215 MPa

Show Material materials with Yield strength Rp1.0 of 215 MPa

300.0 °C

205 MPa

Show Material materials with Yield strength Rp1.0 of 205 MPa

350.0 °C

195 MPa

Show Material materials with Yield strength Rp1.0 of 195 MPa

400.0 °C

190 MPa

Show Material materials with Yield strength Rp1.0 of 190 MPa

450.0 °C

160 MPa

Show Material materials with Yield strength Rp1.0 of 160 MPa

500.0 °C

150 MPa

Show Material materials with Yield strength Rp1.0 of 150 MPa

550.0 °C

135 MPa

Show Material materials with Yield strength Rp1.0 of 135 MPa

Unlock all property charts

Yield strength Rp1.0, transverse

20.0 °C

320 - 340 MPa

Show Material materials with Yield strength Rp1.0, transverse of 320 - 340 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

-100.0 °C

1.49E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.49E-5 1/K

20.0 °C

1.61E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.61E-5 1/K

100.0 °C

1.58E-5 - 1.67E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.58E-5 - 1.67E-5 1/K

200.0 °C

1.61E-5 - 1.72E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.61E-5 - 1.72E-5 1/K

300.0 °C

1.65E-5 - 1.77E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.65E-5 - 1.77E-5 1/K

400.0 °C

1.69E-5 - 1.81E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.69E-5 - 1.81E-5 1/K

500.0 °C

1.73E-5 - 1.84E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.73E-5 - 1.84E-5 1/K

600.0 °C

1.88E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.88E-5 1/K

700.0 °C

1.91E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.91E-5 1/K

800.0 °C

1.94E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.94E-5 1/K

900.0 °C

1.97E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.97E-5 1/K

1000.0 °C

2E-5 1/K

Show Material materials with Coefficient of thermal expansion of 2E-5 1/K

Unlock all property charts

Melting point

1230 - 1480 °C

Show Material materials with Melting point of 1230 - 1480 °C

Typical for Austenitic Stainless Steel

Specific heat capacity

-100.0 °C

440 J/(kg·K)

Show Material materials with Specific heat capacity of 440 J/(kg·K)

20.0 °C

450 - 472 J/(kg·K)

Show Material materials with Specific heat capacity of 450 - 472 J/(kg·K)

100.0 °C

487 J/(kg·K)

Show Material materials with Specific heat capacity of 487 J/(kg·K)

200.0 °C

503 J/(kg·K)

Show Material materials with Specific heat capacity of 503 J/(kg·K)

300.0 °C

512 J/(kg·K)

Show Material materials with Specific heat capacity of 512 J/(kg·K)

400.0 °C

520 J/(kg·K)

Show Material materials with Specific heat capacity of 520 J/(kg·K)

500.0 °C

530 J/(kg·K)

Show Material materials with Specific heat capacity of 530 J/(kg·K)

600.0 °C

541 J/(kg·K)

Show Material materials with Specific heat capacity of 541 J/(kg·K)

700.0 °C

551 J/(kg·K)

Show Material materials with Specific heat capacity of 551 J/(kg·K)

800.0 °C

559 J/(kg·K)

Show Material materials with Specific heat capacity of 559 J/(kg·K)

900.0 °C

565 J/(kg·K)

Show Material materials with Specific heat capacity of 565 J/(kg·K)

1000.0 °C

571 J/(kg·K)

Show Material materials with Specific heat capacity of 571 J/(kg·K)

Unlock all property charts

Thermal conductivity

20.0 °C

11.9 - 12 W/(m·K)

Show Material materials with Thermal conductivity of 11.9 - 12 W/(m·K)

100.0 °C

13.3 W/(m·K)

Show Material materials with Thermal conductivity of 13.3 W/(m·K)

200.0 °C

15.1 W/(m·K)

Show Material materials with Thermal conductivity of 15.1 W/(m·K)

300.0 °C

16.7 W/(m·K)

Show Material materials with Thermal conductivity of 16.7 W/(m·K)

400.0 °C

18.3 W/(m·K)

Show Material materials with Thermal conductivity of 18.3 W/(m·K)

500.0 °C

19.8 W/(m·K)

Show Material materials with Thermal conductivity of 19.8 W/(m·K)

600.0 °C

21.3 W/(m·K)

Show Material materials with Thermal conductivity of 21.3 W/(m·K)

700.0 °C

22.8 W/(m·K)

Show Material materials with Thermal conductivity of 22.8 W/(m·K)

800.0 °C

24.3 W/(m·K)

Show Material materials with Thermal conductivity of 24.3 W/(m·K)

900.0 °C

25.7 W/(m·K)

Show Material materials with Thermal conductivity of 25.7 W/(m·K)

1000.0 °C

27.1 W/(m·K)

Show Material materials with Thermal conductivity of 27.1 W/(m·K)

Unlock all property charts

Thermal diffusivity

20.0 °C

3.3 mm²/s

Show Material materials with Thermal diffusivity of 3.3 mm²/s

100.0 °C

3.4 mm²/s

Show Material materials with Thermal diffusivity of 3.4 mm²/s

200.0 °C

3.7 mm²/s

Show Material materials with Thermal diffusivity of 3.7 mm²/s

300.0 °C

4.1 mm²/s

Show Material materials with Thermal diffusivity of 4.1 mm²/s

400.0 °C

4.3 mm²/s

Show Material materials with Thermal diffusivity of 4.3 mm²/s

500.0 °C

4.5 mm²/s

Show Material materials with Thermal diffusivity of 4.5 mm²/s

600.0 °C

4.7 mm²/s

Show Material materials with Thermal diffusivity of 4.7 mm²/s

700.0 °C

5 mm²/s

Show Material materials with Thermal diffusivity of 5 mm²/s

800.0 °C

5.4 mm²/s

Show Material materials with Thermal diffusivity of 5.4 mm²/s

900.0 °C

5.7 mm²/s

Show Material materials with Thermal diffusivity of 5.7 mm²/s

1000.0 °C

5.8 mm²/s

Show Material materials with Thermal diffusivity of 5.8 mm²/s

Unlock all property charts

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

9.59E-7 - 1E-6 Ω·m

Show Material materials with Electrical resistivity of 9.59E-7 - 1E-6 Ω·m

100.0 °C

1.01E-6 Ω·m

Show Material materials with Electrical resistivity of 1.01E-6 Ω·m

200.0 °C

1.05E-6 Ω·m

Show Material materials with Electrical resistivity of 1.05E-6 Ω·m

300.0 °C

1.1E-6 Ω·m

Show Material materials with Electrical resistivity of 1.1E-6 Ω·m

400.0 °C

1.13E-6 Ω·m

Show Material materials with Electrical resistivity of 1.13E-6 Ω·m

500.0 °C

1.17E-6 Ω·m

Show Material materials with Electrical resistivity of 1.17E-6 Ω·m

600.0 °C

1.19E-6 Ω·m

Show Material materials with Electrical resistivity of 1.19E-6 Ω·m

700.0 °C

1.22E-6 Ω·m

Show Material materials with Electrical resistivity of 1.22E-6 Ω·m

800.0 °C

1.24E-6 Ω·m

Show Material materials with Electrical resistivity of 1.24E-6 Ω·m

900.0 °C

1.26E-6 Ω·m

Show Material materials with Electrical resistivity of 1.26E-6 Ω·m

1000.0 °C

1.28E-6 Ω·m

Show Material materials with Electrical resistivity of 1.28E-6 Ω·m

Unlock all property charts

Chemical properties

PropertyValue

Carbon

0.02 %

Show Material materials with Carbon of 0.02 %

Chromium

19 - 21 %

Show Material materials with Chromium of 19 - 21 %

Copper

0.5 - 1.5 %

Show Material materials with Copper of 0.5 - 1.5 %

Manganese

1 %

Show Material materials with Manganese of 1 %

Molybdenum

6 - 7 %

Show Material materials with Molybdenum of 6 - 7 %

Nickel

24 - 26 %

Show Material materials with Nickel of 24 - 26 %

Nitrogen

0.15 - 0.25 %

Show Material materials with Nitrogen of 0.15 - 0.25 %

Phosphorus

0.03 %

Show Material materials with Phosphorus of 0.03 %

Silicon

0.5 %

Show Material materials with Silicon of 0.5 %

Sulfur

0.01 %

Show Material materials with Sulfur of 0.01 %

Do you have a technical question or need more information about this material?

Post it as a comment below and receive answers from engineers and other community members.