The material X10CrAlSi25, mat. No 1.4762 is a heat-resistant steel of max. scaling resistance at 1150 °C (highest application temp. in air). The steel is highly resistant to oxidizing, sulfureous athmosphere. Low resistance in nitrogenous, oxygen deficient gases. The temp. limit in permanent operation accounts for 1000 °C: The steel has 3 embrittlement spans: 475 °C, 600 to 850 °C and above 900 °C. Application for oven components, gadgetries, annealing boxes for components of low mechanical load.

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

7.47 - 7.7 g/cm³

Show Material materials with Density of 7.47 - 7.7 g/cm³

Mechanical

PropertyTemperatureValueComment

Elastic modulus

20.0 °C

218 GPa

Show Material materials with Elastic modulus of 218 GPa

100.0 °C

213 GPa

Show Material materials with Elastic modulus of 213 GPa

200.0 °C

206 GPa

Show Material materials with Elastic modulus of 206 GPa

300.0 °C

198 GPa

Show Material materials with Elastic modulus of 198 GPa

400.0 °C

190 GPa

Show Material materials with Elastic modulus of 190 GPa

500.0 °C

180 GPa

Show Material materials with Elastic modulus of 180 GPa

600.0 °C

167 GPa

Show Material materials with Elastic modulus of 167 GPa

700.0 °C

150 GPa

Show Material materials with Elastic modulus of 150 GPa

Elongation

20.0 °C

10 - 15 %

Show Material materials with Elongation of 10 - 15 %

Elongation A80

20.0 °C

13 %

Show Material materials with Elongation A80 of 13 %

Hardness, Brinell

20.0 °C

223 [-]

Show Material materials with Hardness, Brinell of 223 [-]

Poisson's ratio

23.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

Typical for Ferritic Stainless Steel

Shear modulus

23.0 °C

77 GPa

Show Material materials with Shear modulus of 77 GPa

Typical for Ferritic Stainless Steel

Tensile strength

20.0 °C

520 - 720 MPa

Show Material materials with Tensile strength of 520 - 720 MPa

Yield strength Rp0.2

20.0 °C

280 MPa

Show Material materials with Yield strength Rp0.2 of 280 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

20.0 °C

9.9E-6 1/K

Show Material materials with Coefficient of thermal expansion of 9.9E-6 1/K

100.0 °C

1.03E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.03E-5 1/K

200.0 °C

1.05E-5 - 1.07E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.05E-5 - 1.07E-5 1/K

300.0 °C

1.11E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.11E-5 1/K

400.0 °C

1.15E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.15E-5 1/K

500.0 °C

1.18E-5 - 1.2E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.18E-5 - 1.2E-5 1/K

600.0 °C

1.2E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.2E-5 1/K

700.0 °C

1.24E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.24E-5 1/K

800.0 °C

1.2E-5 - 1.29E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.2E-5 - 1.29E-5 1/K

900.0 °C

1.34E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.34E-5 1/K

1000.0 °C

1.35E-5 - 1.4E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.35E-5 - 1.4E-5 1/K

Unlock all property charts

Max service temperature, long

0 - 1000 °C

Show Material materials with Max service temperature, long of 0 - 1000 °C

Melting point

1425 - 1530 °C

Show Material materials with Melting point of 1425 - 1530 °C

Typical for Ferritic Stainless Steel

Specific heat capacity

20.0 °C

457 - 500 J/(kg·K)

Show Material materials with Specific heat capacity of 457 - 500 J/(kg·K)

100.0 °C

498 J/(kg·K)

Show Material materials with Specific heat capacity of 498 J/(kg·K)

200.0 °C

534 J/(kg·K)

Show Material materials with Specific heat capacity of 534 J/(kg·K)

300.0 °C

555 J/(kg·K)

Show Material materials with Specific heat capacity of 555 J/(kg·K)

400.0 °C

577 J/(kg·K)

Show Material materials with Specific heat capacity of 577 J/(kg·K)

500.0 °C

605 J/(kg·K)

Show Material materials with Specific heat capacity of 605 J/(kg·K)

600.0 °C

648 J/(kg·K)

Show Material materials with Specific heat capacity of 648 J/(kg·K)

700.0 °C

656 J/(kg·K)

Show Material materials with Specific heat capacity of 656 J/(kg·K)

800.0 °C

657 J/(kg·K)

Show Material materials with Specific heat capacity of 657 J/(kg·K)

900.0 °C

657 J/(kg·K)

Show Material materials with Specific heat capacity of 657 J/(kg·K)

1000.0 °C

658 J/(kg·K)

Show Material materials with Specific heat capacity of 658 J/(kg·K)

Unlock all property charts

Thermal conductivity

20.0 °C

14.2 - 17 W/(m·K)

Show Material materials with Thermal conductivity of 14.2 - 17 W/(m·K)

100.0 °C

15.5 W/(m·K)

Show Material materials with Thermal conductivity of 15.5 W/(m·K)

200.0 °C

17 W/(m·K)

Show Material materials with Thermal conductivity of 17 W/(m·K)

300.0 °C

18.3 W/(m·K)

Show Material materials with Thermal conductivity of 18.3 W/(m·K)

400.0 °C

19.7 W/(m·K)

Show Material materials with Thermal conductivity of 19.7 W/(m·K)

500.0 °C

20.9 - 23 W/(m·K)

Show Material materials with Thermal conductivity of 20.9 - 23 W/(m·K)

600.0 °C

21.9 W/(m·K)

Show Material materials with Thermal conductivity of 21.9 W/(m·K)

700.0 °C

23.2 W/(m·K)

Show Material materials with Thermal conductivity of 23.2 W/(m·K)

800.0 °C

24.6 W/(m·K)

Show Material materials with Thermal conductivity of 24.6 W/(m·K)

900.0 °C

26.1 W/(m·K)

Show Material materials with Thermal conductivity of 26.1 W/(m·K)

1000.0 °C

27.5 W/(m·K)

Show Material materials with Thermal conductivity of 27.5 W/(m·K)

Unlock all property charts

Thermal diffusivity

20.0 °C

4.2 mm²/s

Show Material materials with Thermal diffusivity of 4.2 mm²/s

100.0 °C

3.9 mm²/s

Show Material materials with Thermal diffusivity of 3.9 mm²/s

200.0 °C

3.9 mm²/s

Show Material materials with Thermal diffusivity of 3.9 mm²/s

300.0 °C

4 mm²/s

Show Material materials with Thermal diffusivity of 4 mm²/s

400.0 °C

4.1 mm²/s

Show Material materials with Thermal diffusivity of 4.1 mm²/s

500.0 °C

3.2 mm²/s

Show Material materials with Thermal diffusivity of 3.2 mm²/s

600.0 °C

3.9 mm²/s

Show Material materials with Thermal diffusivity of 3.9 mm²/s

700.0 °C

4.8 mm²/s

Show Material materials with Thermal diffusivity of 4.8 mm²/s

800.0 °C

5.1 mm²/s

Show Material materials with Thermal diffusivity of 5.1 mm²/s

900.0 °C

5.5 mm²/s

Show Material materials with Thermal diffusivity of 5.5 mm²/s

1000.0 °C

5.7 mm²/s

Show Material materials with Thermal diffusivity of 5.7 mm²/s

Unlock all property charts

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

1.02E-6 - 1.1E-6 Ω·m

Show Material materials with Electrical resistivity of 1.02E-6 - 1.1E-6 Ω·m

100.0 °C

1.05E-6 Ω·m

Show Material materials with Electrical resistivity of 1.05E-6 Ω·m

200.0 °C

1.09E-6 Ω·m

Show Material materials with Electrical resistivity of 1.09E-6 Ω·m

300.0 °C

1.12E-6 Ω·m

Show Material materials with Electrical resistivity of 1.12E-6 Ω·m

400.0 °C

1.16E-6 Ω·m

Show Material materials with Electrical resistivity of 1.16E-6 Ω·m

500.0 °C

1.2E-6 Ω·m

Show Material materials with Electrical resistivity of 1.2E-6 Ω·m

600.0 °C

1.24E-6 Ω·m

Show Material materials with Electrical resistivity of 1.24E-6 Ω·m

700.0 °C

1.27E-6 Ω·m

Show Material materials with Electrical resistivity of 1.27E-6 Ω·m

800.0 °C

1.28E-6 Ω·m

Show Material materials with Electrical resistivity of 1.28E-6 Ω·m

900.0 °C

1.3E-6 Ω·m

Show Material materials with Electrical resistivity of 1.3E-6 Ω·m

1000.0 °C

1.31E-6 Ω·m

Show Material materials with Electrical resistivity of 1.31E-6 Ω·m

Unlock all property charts

Chemical properties

PropertyValue

Aluminium

1.2 - 1.7 %

Show Material materials with Aluminium of 1.2 - 1.7 %

Carbon

0.12 %

Show Material materials with Carbon of 0.12 %

Chromium

23 - 26 %

Show Material materials with Chromium of 23 - 26 %

Manganese

1 %

Show Material materials with Manganese of 1 %

Phosphorus

0.04 %

Show Material materials with Phosphorus of 0.04 %

Silicon

0.7 - 1.4 %

Show Material materials with Silicon of 0.7 - 1.4 %

Sulfur

0.015 %