EN 10095 Grade X12NiCrSi35-16 solution annealed (+AT)

Want to keep this datasheet? Save it now in your required format

Description

For components in furnace and apparatus engineering for high working temperatures, no embrittlement risk in the critical temperature range from 600 to 850 °C. (highest application temperature in air 1100 °C).

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

7.98 - 8 g/cm³

Show Material materials with Density of 7.98 - 8 g/cm³

Mechanical

PropertyTemperatureValueComment

Elastic modulus

-100.0 °C

201 GPa

Show Material materials with Elastic modulus of 201 GPa

20.0 °C

194 GPa

Show Material materials with Elastic modulus of 194 GPa

100.0 °C

189 GPa

Show Material materials with Elastic modulus of 189 GPa

200.0 °C

183 GPa

Show Material materials with Elastic modulus of 183 GPa

300.0 °C

177 GPa

Show Material materials with Elastic modulus of 177 GPa

400.0 °C

170 GPa

Show Material materials with Elastic modulus of 170 GPa

500.0 °C

163 GPa

Show Material materials with Elastic modulus of 163 GPa

600.0 °C

156 GPa

Show Material materials with Elastic modulus of 156 GPa

700.0 °C

149 GPa

Show Material materials with Elastic modulus of 149 GPa

800.0 °C

141 GPa

Show Material materials with Elastic modulus of 141 GPa

900.0 °C

134 GPa

Show Material materials with Elastic modulus of 134 GPa

1000.0 °C

127 GPa

Show Material materials with Elastic modulus of 127 GPa

Elongation

20.0 °C

30 %

Show Material materials with Elongation of 30 %

Elongation A80

20.0 °C

28 %

Show Material materials with Elongation A80 of 28 %

Hardness, Brinell

20.0 °C

223 [-]

Show Material materials with Hardness, Brinell of 223 [-]

Poisson's ratio

23.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

Typical for Steel

Tensile strength

20.0 °C

550 - 750 MPa

Show Material materials with Tensile strength of 550 - 750 MPa

Yield strength Rp0.2

20.0 °C

230 MPa

Show Material materials with Yield strength Rp0.2 of 230 MPa

Yield strength Rp1.0

20.0 °C

270 MPa

Show Material materials with Yield strength Rp1.0 of 270 MPa

Thermal

PropertyTemperatureValue

Coefficient of thermal expansion

-100.0 °C

1.36E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.36E-5 1/K

20.0 °C

1.46E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.46E-5 1/K

100.0 °C

1.51E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.51E-5 1/K

200.0 °C

1.5E-5 - 1.57E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.5E-5 - 1.57E-5 1/K

300.0 °C

1.62E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.62E-5 1/K

400.0 °C

1.6E-5 - 1.66E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.6E-5 - 1.66E-5 1/K

500.0 °C

1.7E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.7E-5 1/K

600.0 °C

1.7E-5 - 1.74E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.7E-5 - 1.74E-5 1/K

700.0 °C

1.77E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.77E-5 1/K

800.0 °C

1.75E-5 - 1.8E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.75E-5 - 1.8E-5 1/K

900.0 °C

1.83E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.83E-5 1/K

1000.0 °C

1.85E-5 - 1.86E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.85E-5 - 1.86E-5 1/K

Unlock all property charts

Max service temperature, long

0 - 1100 °C

Show Material materials with Max service temperature, long of 0 - 1100 °C

Specific heat capacity

-100.0 °C

440 J/(kg·K)

Show Material materials with Specific heat capacity of 440 J/(kg·K)

20.0 °C

472 - 550 J/(kg·K)

Show Material materials with Specific heat capacity of 472 - 550 J/(kg·K)

100.0 °C

487 J/(kg·K)

Show Material materials with Specific heat capacity of 487 J/(kg·K)

200.0 °C

503 J/(kg·K)

Show Material materials with Specific heat capacity of 503 J/(kg·K)

300.0 °C

512 J/(kg·K)

Show Material materials with Specific heat capacity of 512 J/(kg·K)

400.0 °C

520 J/(kg·K)

Show Material materials with Specific heat capacity of 520 J/(kg·K)

500.0 °C

530 J/(kg·K)

Show Material materials with Specific heat capacity of 530 J/(kg·K)

600.0 °C

541 J/(kg·K)

Show Material materials with Specific heat capacity of 541 J/(kg·K)

700.0 °C

551 J/(kg·K)

Show Material materials with Specific heat capacity of 551 J/(kg·K)

800.0 °C

559 J/(kg·K)

Show Material materials with Specific heat capacity of 559 J/(kg·K)

900.0 °C

565 J/(kg·K)

Show Material materials with Specific heat capacity of 565 J/(kg·K)

1000.0 °C

571 J/(kg·K)

Show Material materials with Specific heat capacity of 571 J/(kg·K)

Unlock all property charts

Thermal conductivity

20.0 °C

11.4 - 12.5 W/(m·K)

Show Material materials with Thermal conductivity of 11.4 - 12.5 W/(m·K)

100.0 °C

12.8 W/(m·K)

Show Material materials with Thermal conductivity of 12.8 W/(m·K)

200.0 °C

14.6 W/(m·K)

Show Material materials with Thermal conductivity of 14.6 W/(m·K)

300.0 °C

16.3 W/(m·K)

Show Material materials with Thermal conductivity of 16.3 W/(m·K)

400.0 °C

17.9 W/(m·K)

Show Material materials with Thermal conductivity of 17.9 W/(m·K)

500.0 °C

17 - 19.5 W/(m·K)

Show Material materials with Thermal conductivity of 17 - 19.5 W/(m·K)

600.0 °C

21 W/(m·K)

Show Material materials with Thermal conductivity of 21 W/(m·K)

700.0 °C

22.6 W/(m·K)

Show Material materials with Thermal conductivity of 22.6 W/(m·K)

800.0 °C

24.1 W/(m·K)

Show Material materials with Thermal conductivity of 24.1 W/(m·K)

900.0 °C

25.6 W/(m·K)

Show Material materials with Thermal conductivity of 25.6 W/(m·K)

1000.0 °C

27 W/(m·K)

Show Material materials with Thermal conductivity of 27 W/(m·K)

Unlock all property charts

Thermal diffusivity

20.0 °C

3 mm²/s

Show Material materials with Thermal diffusivity of 3 mm²/s

100.0 °C

3.2 mm²/s

Show Material materials with Thermal diffusivity of 3.2 mm²/s

200.0 °C

3.5 mm²/s

Show Material materials with Thermal diffusivity of 3.5 mm²/s

300.0 °C

4 mm²/s

Show Material materials with Thermal diffusivity of 4 mm²/s

400.0 °C

4.1 mm²/s

Show Material materials with Thermal diffusivity of 4.1 mm²/s

500.0 °C

4.3 mm²/s

Show Material materials with Thermal diffusivity of 4.3 mm²/s

600.0 °C

4.5 mm²/s

Show Material materials with Thermal diffusivity of 4.5 mm²/s

700.0 °C

4.8 mm²/s

Show Material materials with Thermal diffusivity of 4.8 mm²/s

800.0 °C

5.2 mm²/s

Show Material materials with Thermal diffusivity of 5.2 mm²/s

900.0 °C

5.5 mm²/s

Show Material materials with Thermal diffusivity of 5.5 mm²/s

1000.0 °C

5.6 mm²/s

Show Material materials with Thermal diffusivity of 5.6 mm²/s

Unlock all property charts

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

1E-6 - 1.04E-6 Ω·m

Show Material materials with Electrical resistivity of 1E-6 - 1.04E-6 Ω·m

100.0 °C

1.07E-6 Ω·m

Show Material materials with Electrical resistivity of 1.07E-6 Ω·m

200.0 °C

1.11E-6 Ω·m

Show Material materials with Electrical resistivity of 1.11E-6 Ω·m

300.0 °C

1.14E-6 Ω·m

Show Material materials with Electrical resistivity of 1.14E-6 Ω·m

400.0 °C

1.17E-6 Ω·m

Show Material materials with Electrical resistivity of 1.17E-6 Ω·m

500.0 °C

1.19E-6 Ω·m

Show Material materials with Electrical resistivity of 1.19E-6 Ω·m

600.0 °C

1.22E-6 Ω·m

Show Material materials with Electrical resistivity of 1.22E-6 Ω·m

700.0 °C

1.23E-6 Ω·m

Show Material materials with Electrical resistivity of 1.23E-6 Ω·m

800.0 °C

1.25E-6 Ω·m

Show Material materials with Electrical resistivity of 1.25E-6 Ω·m

900.0 °C

1.57E-6 Ω·m

Show Material materials with Electrical resistivity of 1.57E-6 Ω·m

1000.0 °C

1.29E-6 Ω·m

Show Material materials with Electrical resistivity of 1.29E-6 Ω·m

Unlock all property charts

Chemical properties

PropertyValue

Carbon

0.15 %

Show Material materials with Carbon of 0.15 %

Chromium

15 - 17 %

Show Material materials with Chromium of 15 - 17 %

Manganese

2 %

Show Material materials with Manganese of 2 %

Nickel

33 - 37 %

Show Material materials with Nickel of 33 - 37 %

Nitrogen

0.11 %

Show Material materials with Nitrogen of 0.11 %

Phosphorus

0.05 %

Show Material materials with Phosphorus of 0.05 %

Silicon

1 - 2 %

Show Material materials with Silicon of 1 - 2 %

Sulfur

0.015 %

Show Material materials with Sulfur of 0.015 %