EN 10095 Grade X10NiCrSiNb35-22 solution annealed (+AT)

Want to keep this datasheet? Save it now in your required format

Description

Steel X10NiCrSiNb35-22 shows a highest application temperature of up to 1100 °C in air.

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

8 g/cm³

Show Material materials with Density of 8 g/cm³

Mechanical

PropertyTemperatureValueComment

Elastic modulus

23.0 °C

200 GPa

Show Material materials with Elastic modulus of 200 GPa

Typical for Duplex Stainless Steel

Elongation

20.0 °C

40 %

Show Material materials with Elongation of 40 %

Hardness, Brinell

20.0 °C

200 [-]

Show Material materials with Hardness, Brinell of 200 [-]

Poisson's ratio

23.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

Typical for Duplex Stainless Steel

Shear modulus

23.0 °C

77 GPa

Show Material materials with Shear modulus of 77 GPa

Typical for Duplex Stainless Steel

Tensile strength

20.0 °C

500 - 650 MPa

Show Material materials with Tensile strength of 500 - 650 MPa

Yield strength Rp0.2

20.0 °C

270 MPa

Show Material materials with Yield strength Rp0.2 of 270 MPa

Yield strength Rp1.0

20.0 °C

300 MPa

Show Material materials with Yield strength Rp1.0 of 300 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

200.0 °C

1.55E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.55E-5 1/K

400.0 °C

1.6E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.6E-5 1/K

600.0 °C

1.7E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.7E-5 1/K

800.0 °C

1.77E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.77E-5 1/K

1000.0 °C

1.8E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.8E-5 1/K

Max service temperature

300 °C

Show Material materials with Max service temperature of 300 °C

Typical for Duplex Stainless Steel

Max service temperature, long

0 - 1100 °C

Show Material materials with Max service temperature, long of 0 - 1100 °C

Melting point

1375 - 1450 °C

Show Material materials with Melting point of 1375 - 1450 °C

Typical for Duplex Stainless Steel

Specific heat capacity

20.0 °C

460 J/(kg·K)

Show Material materials with Specific heat capacity of 460 J/(kg·K)

Thermal conductivity

20.0 °C

12 W/(m·K)

Show Material materials with Thermal conductivity of 12 W/(m·K)

500.0 °C

19.5 W/(m·K)

Show Material materials with Thermal conductivity of 19.5 W/(m·K)

Unlock all property charts

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

1E-6 Ω·m

Show Material materials with Electrical resistivity of 1E-6 Ω·m

Chemical properties

PropertyValue

Carbon

0.15 %

Show Material materials with Carbon of 0.15 %

Chromium

20 - 23 %

Show Material materials with Chromium of 20 - 23 %

Manganese

2 %

Show Material materials with Manganese of 2 %

Nickel

33 - 37 %

Show Material materials with Nickel of 33 - 37 %

Niobium

1 - 1.5 %

Show Material materials with Niobium of 1 - 1.5 %

Nitrogen

0.11 %

Show Material materials with Nitrogen of 0.11 %

Phosphorus

0.03 %

Show Material materials with Phosphorus of 0.03 %

Silicon

1 - 2 %

Show Material materials with Silicon of 1 - 2 %

Sulfur

0.015 %

Show Material materials with Sulfur of 0.015 %