Material GP240GH is equivalent to trademark GS-C 25 acc. to DIN 17245-87. It is used at room temperature and increased temperatures. The DIN-make shows only a low long-term thermal resistance and is therefore applicated in the range of the hot elastic limit. The well weldable material is used for turbine parts and pressure vessels at temperatures from 300 to 450 °C and mean pressure, e.g. for casings and fittings.

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

7.8 g/cm³

Show Material materials with Density of 7.8 g/cm³

Mechanical

PropertyTemperatureValueComment

Elastic modulus

20.0 °C

211 GPa

Show Material materials with Elastic modulus of 211 GPa

100.0 °C

204 GPa

Show Material materials with Elastic modulus of 204 GPa

200.0 °C

196 GPa

Show Material materials with Elastic modulus of 196 GPa

300.0 °C

186 GPa

Show Material materials with Elastic modulus of 186 GPa

400.0 °C

177 GPa

Show Material materials with Elastic modulus of 177 GPa

500.0 °C

164 GPa

Show Material materials with Elastic modulus of 164 GPa

600.0 °C

127 GPa

Show Material materials with Elastic modulus of 127 GPa

Elongation

20.0 °C

22 %

Show Material materials with Elongation of 22 %

Poisson's ratio

23.0 °C

0.29 [-]

Show Material materials with Poisson's ratio of 0.29 [-]

Typical for Low Carbon Steel

Shear modulus

23.0 °C

82 GPa

Show Material materials with Shear modulus of 82 GPa

Typical for Low Carbon Steel

Tensile strength

20.0 °C

420 - 600 MPa

Show Material materials with Tensile strength of 420 - 600 MPa

Yield strength Rp0.2

20.0 °C

240 MPa

Show Material materials with Yield strength Rp0.2 of 240 MPa

100.0 °C

210 MPa

Show Material materials with Yield strength Rp0.2 of 210 MPa

200.0 °C

175 MPa

Show Material materials with Yield strength Rp0.2 of 175 MPa

300.0 °C

145 MPa

Show Material materials with Yield strength Rp0.2 of 145 MPa

350.0 °C

135 MPa

Show Material materials with Yield strength Rp0.2 of 135 MPa

400.0 °C

130 MPa

Show Material materials with Yield strength Rp0.2 of 130 MPa

450.0 °C

125 MPa

Show Material materials with Yield strength Rp0.2 of 125 MPa

Unlock all property charts

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

100.0 °C

1.22E-5 - 1.26E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.22E-5 - 1.26E-5 1/K

200.0 °C

1.29E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.29E-5 1/K

300.0 °C

1.34E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.34E-5 1/K

400.0 °C

1.39E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.39E-5 1/K

500.0 °C

1.4E-5 - 1.43E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.4E-5 - 1.43E-5 1/K

600.0 °C

1.46E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.46E-5 1/K

Unlock all property charts

Max service temperature

500 °C

Show Material materials with Max service temperature of 500 °C

Typical for Carbon Steel

Max service temperature, long

300 - 610 °C

Show Material materials with Max service temperature, long of 300 - 610 °C

Melting point

1480 - 1526 °C

Show Material materials with Melting point of 1480 - 1526 °C

Typical for Low Carbon Steel

Specific heat capacity

20.0 °C

460 J/(kg·K)

Show Material materials with Specific heat capacity of 460 J/(kg·K)

Thermal conductivity

20.0 °C

50 W/(m·K)

Show Material materials with Thermal conductivity of 50 W/(m·K)

50.0 °C

45 W/(m·K)

Show Material materials with Thermal conductivity of 45 W/(m·K)

300.0 °C

46 W/(m·K)

Show Material materials with Thermal conductivity of 46 W/(m·K)

400.0 °C

42 W/(m·K)

Show Material materials with Thermal conductivity of 42 W/(m·K)

500.0 °C

38 W/(m·K)

Show Material materials with Thermal conductivity of 38 W/(m·K)

600.0 °C

34 W/(m·K)

Show Material materials with Thermal conductivity of 34 W/(m·K)

Unlock all property charts

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

1.6E-7 Ω·m

Show Material materials with Electrical resistivity of 1.6E-7 Ω·m

Magnetic

PropertyValueComment

Curie temperature

770 °C

Show Material materials with Curie temperature of 770 °C

Typical for Low Carbon Steel

Chemical properties

PropertyValue

Carbon

0.18 - 0.23 %

Show Material materials with Carbon of 0.18 - 0.23 %

Chromium

0.3 %

Show Material materials with Chromium of 0.3 %

Copper

0.3 %

Show Material materials with Copper of 0.3 %

Manganese

0.5 - 1.2 %

Show Material materials with Manganese of 0.5 - 1.2 %

Molybdenum

0.12 %

Show Material materials with Molybdenum of 0.12 %

Nickel

0.4 %

Show Material materials with Nickel of 0.4 %

Phosphorus

0.03 %

Show Material materials with Phosphorus of 0.03 %

Silicon

0.6 %

Show Material materials with Silicon of 0.6 %

Sulfur

0.02 %

Show Material materials with Sulfur of 0.02 %

Vanadium

0.03 %

Show Material materials with Vanadium of 0.03 %