Material G9Ni10 is used for low temperatures up to approx. -70 °C.

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

7.85 g/cm³

Show Material materials with Density of 7.85 g/cm³

Mechanical

PropertyTemperatureValueComment

Elastic modulus

23.0 °C

200 - 215 GPa

Show Material materials with Elastic modulus of 200 - 215 GPa

Typical for Nickel Steel

Elongation

20.0 °C

24 %

Show Material materials with Elongation of 24 %

Poisson's ratio

23.0 °C

0.29 [-]

Show Material materials with Poisson's ratio of 0.29 [-]

Typical for Nickel Steel

Shear modulus

23.0 °C

76 GPa

Show Material materials with Shear modulus of 76 GPa

Typical for Nickel Steel

Tensile strength

20.0 °C

480 - 630 MPa

Show Material materials with Tensile strength of 480 - 630 MPa

Yield strength Rp0.2

20.0 °C

280 MPa

Show Material materials with Yield strength Rp0.2 of 280 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

100.0 °C

1.18E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.18E-5 1/K

300.0 °C

1.24E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.24E-5 1/K

500.0 °C

1.36E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.36E-5 1/K

Melting point

1316 - 1595 °C

Show Material materials with Melting point of 1316 - 1595 °C

Typical for Nickel Steel

Specific heat capacity

20.0 °C

460 J/(kg·K)

Show Material materials with Specific heat capacity of 460 J/(kg·K)

Thermal conductivity

50.0 °C

36 W/(m·K)

Show Material materials with Thermal conductivity of 36 W/(m·K)

Chemical properties

PropertyValue

Carbon

0.06 - 0.12 %

Show Material materials with Carbon of 0.06 - 0.12 %

Chromium

0.3 %

Show Material materials with Chromium of 0.3 %

Copper

0.3 %

Show Material materials with Copper of 0.3 %

Manganese

0.5 - 0.8 %

Show Material materials with Manganese of 0.5 - 0.8 %

Molybdenum

0.2 %

Show Material materials with Molybdenum of 0.2 %

Nickel

2 - 3 %

Show Material materials with Nickel of 2 - 3 %

Phosphorus

0.02 %

Show Material materials with Phosphorus of 0.02 %

Silicon

0.6 %

Show Material materials with Silicon of 0.6 %

Sulfur

0.015 %

Show Material materials with Sulfur of 0.015 %

Vanadium

0.05 %

Show Material materials with Vanadium of 0.05 %