EN 10216-2 Grade 11CrMo9-10 quenched and tempered (+QT)

View suppliers (5)
Want to keep this datasheet? Save it now in your required format

Description

Seamless tubes of the high-temperature 11CrMo9-10 are used in steam boiler and pipeline construction, pressure vessel and apparatus engineering, especially in chemical industry and power station construction at temperatures from approx. 200 °C to maximum 400 °C and simultaneously high pressures. The total load and the special scaling circumstances can decrease or increase the temperature limit. Weldability is available.

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

"Typical" values were obtained via a literature search. "Predicted" values were imputed via artificial intelligence technology. While we have placed significant efforts in ensuring data accuracy, "typical" and "predicted" data should be considered indicative and verified by appropriate material testing. Please do contact us if additional information on the the predicted data method is required.
All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueComment

Density

23.0 °C

7.8 - 7.9 g/cm³

Show Material materials with Density of 7.8 - 7.9 g/cm³

Typical for Chromium Molybdenum Steel

Mechanical

PropertyTemperatureValueComment

Elastic modulus

23.0 °C

200 - 215 GPa

Show Material materials with Elastic modulus of 200 - 215 GPa

Typical for Chromium Molybdenum Steel

Elongation

20.0 °C

20 %

Show Material materials with Elongation of 20 %

Elongation, transverse

20.0 °C

18 %

Show Material materials with Elongation, transverse of 18 %

Poisson's ratio

23.0 °C

0.29 [-]

Show Material materials with Poisson's ratio of 0.29 [-]

Typical for Chromium Molybdenum Steel

Tensile strength

20.0 °C

540 - 680 MPa

Show Material materials with Tensile strength of 540 - 680 MPa

Tensile strength, transverse

20.0 °C

540 - 680 MPa

Show Material materials with Tensile strength, transverse of 540 - 680 MPa

Yield strength Rp0.2

20.0 °C

355 MPa

Show Material materials with Yield strength Rp0.2 of 355 MPa

100.0 °C

323 MPa

Show Material materials with Yield strength Rp0.2 of 323 MPa

150.0 °C

312 MPa

Show Material materials with Yield strength Rp0.2 of 312 MPa

200.0 °C

304 MPa

Show Material materials with Yield strength Rp0.2 of 304 MPa

250.0 °C

296 MPa

Show Material materials with Yield strength Rp0.2 of 296 MPa

300.0 °C

289 MPa

Show Material materials with Yield strength Rp0.2 of 289 MPa

350.0 °C

280 MPa

Show Material materials with Yield strength Rp0.2 of 280 MPa

400.0 °C

275 MPa

Show Material materials with Yield strength Rp0.2 of 275 MPa

450.0 °C

257 MPa

Show Material materials with Yield strength Rp0.2 of 257 MPa

500.0 °C

239 MPa

Show Material materials with Yield strength Rp0.2 of 239 MPa

Yield strength Rp0.2, transverse

20.0 °C

355 MPa

Show Material materials with Yield strength Rp0.2, transverse of 355 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

23.0 °C

1.1E-5 - 1.4E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.1E-5 - 1.4E-5 1/K

Typical for Chromium Molybdenum Steel

Max service temperature, long

200 - 550 °C

Show Material materials with Max service temperature, long of 200 - 550 °C

Melting point

1382 - 1529 °C

Show Material materials with Melting point of 1382 - 1529 °C

Typical for Chromium Molybdenum Steel

Specific heat capacity

23.0 °C

448 - 502 J/(kg·K)

Show Material materials with Specific heat capacity of 448 - 502 J/(kg·K)

Typical for Chromium Molybdenum Steel

Thermal conductivity

23.0 °C

36 - 43 W/(m·K)

Show Material materials with Thermal conductivity of 36 - 43 W/(m·K)

Typical for Chromium Molybdenum Steel

Chemical properties

PropertyValue

Aluminium

0.04 %

Show Material materials with Aluminium of 0.04 %

Carbon

0.08 - 0.15 %

Show Material materials with Carbon of 0.08 - 0.15 %

Chromium

2 - 2.5 %

Show Material materials with Chromium of 2 - 2.5 %

Copper

0.3 %

Show Material materials with Copper of 0.3 %

Manganese

0.4 - 0.8 %

Show Material materials with Manganese of 0.4 - 0.8 %

Molybdenum

0.9 - 1.1 %

Show Material materials with Molybdenum of 0.9 - 1.1 %

Nickel

0.3 %

Show Material materials with Nickel of 0.3 %

Phosphorus

0.03 %

Show Material materials with Phosphorus of 0.03 %

Silicon

0.5 %

Show Material materials with Silicon of 0.5 %

Sulfur

0.01 - 0.02 %

Show Material materials with Sulfur of 0.01 - 0.02 %