Seamless tubes of the high-temperature 20CrMoV13-5-5 are used in steam boiler and pipeline construction, pressure vessel and apparatus engineering, especially in chemical industry and power station construction at temperatures from approx. 200 °C to maximum 400 °C and simultaneously high pressures. The total load and the special scaling circumstances can decrease or increase the temperature limit. Weldability is available.

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

7.83 g/cm³

Show Material materials with Density of 7.83 g/cm³

Mechanical

PropertyTemperatureValueComment

Elastic modulus

-100.0 °C

217 GPa

Show Material materials with Elastic modulus of 217 GPa

20.0 °C

212 GPa

Show Material materials with Elastic modulus of 212 GPa

100.0 °C

207 GPa

Show Material materials with Elastic modulus of 207 GPa

200.0 °C

199 GPa

Show Material materials with Elastic modulus of 199 GPa

300.0 °C

192 GPa

Show Material materials with Elastic modulus of 192 GPa

400.0 °C

184 GPa

Show Material materials with Elastic modulus of 184 GPa

500.0 °C

175 GPa

Show Material materials with Elastic modulus of 175 GPa

600.0 °C

164 GPa

Show Material materials with Elastic modulus of 164 GPa

Elongation

20.0 °C

16 %

Show Material materials with Elongation of 16 %

Elongation, transverse

20.0 °C

14 %

Show Material materials with Elongation, transverse of 14 %

Poisson's ratio

23.0 °C

0.29 [-]

Show Material materials with Poisson's ratio of 0.29 [-]

Typical for Chromium Molybdenum Steel

Tensile strength

20.0 °C

740 - 880 MPa

Show Material materials with Tensile strength of 740 - 880 MPa

Tensile strength, transverse

20.0 °C

740 - 880 MPa

Show Material materials with Tensile strength, transverse of 740 - 880 MPa

Yield strength Rp0.2

20.0 °C

590 MPa

Show Material materials with Yield strength Rp0.2 of 590 MPa

150.0 °C

575 MPa

Show Material materials with Yield strength Rp0.2 of 575 MPa

200.0 °C

570 MPa

Show Material materials with Yield strength Rp0.2 of 570 MPa

250.0 °C

560 MPa

Show Material materials with Yield strength Rp0.2 of 560 MPa

300.0 °C

550 MPa

Show Material materials with Yield strength Rp0.2 of 550 MPa

350.0 °C

510 MPa

Show Material materials with Yield strength Rp0.2 of 510 MPa

400.0 °C

470 MPa

Show Material materials with Yield strength Rp0.2 of 470 MPa

450.0 °C

420 MPa

Show Material materials with Yield strength Rp0.2 of 420 MPa

500.0 °C

370 MPa

Show Material materials with Yield strength Rp0.2 of 370 MPa

Unlock all property charts

Yield strength Rp0.2, transverse

20.0 °C

590 MPa

Show Material materials with Yield strength Rp0.2, transverse of 590 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

-100.0 °C

1.05E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.05E-5 1/K

20.0 °C

1.15E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.15E-5 1/K

100.0 °C

1.21E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.21E-5 1/K

200.0 °C

1.27E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.27E-5 1/K

300.0 °C

1.32E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.32E-5 1/K

400.0 °C

1.36E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.36E-5 1/K

500.0 °C

1.4E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.4E-5 1/K

600.0 °C

1.44E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.44E-5 1/K

Unlock all property charts

Max service temperature, long

200 - 550 °C

Show Material materials with Max service temperature, long of 200 - 550 °C

Melting point

1382 - 1529 °C

Show Material materials with Melting point of 1382 - 1529 °C

Typical for Chromium Molybdenum Steel

Specific heat capacity

-100.0 °C

423 J/(kg·K)

Show Material materials with Specific heat capacity of 423 J/(kg·K)

20.0 °C

461 J/(kg·K)

Show Material materials with Specific heat capacity of 461 J/(kg·K)

100.0 °C

479 J/(kg·K)

Show Material materials with Specific heat capacity of 479 J/(kg·K)

200.0 °C

499 J/(kg·K)

Show Material materials with Specific heat capacity of 499 J/(kg·K)

300.0 °C

517 J/(kg·K)

Show Material materials with Specific heat capacity of 517 J/(kg·K)

400.0 °C

536 J/(kg·K)

Show Material materials with Specific heat capacity of 536 J/(kg·K)

500.0 °C

558 J/(kg·K)

Show Material materials with Specific heat capacity of 558 J/(kg·K)

600.0 °C

587 J/(kg·K)

Show Material materials with Specific heat capacity of 587 J/(kg·K)

Unlock all property charts

Thermal conductivity

20.0 °C

25.7 W/(m·K)

Show Material materials with Thermal conductivity of 25.7 W/(m·K)

100.0 °C

27.4 W/(m·K)

Show Material materials with Thermal conductivity of 27.4 W/(m·K)

200.0 °C

28.5 W/(m·K)

Show Material materials with Thermal conductivity of 28.5 W/(m·K)

300.0 °C

28.9 W/(m·K)

Show Material materials with Thermal conductivity of 28.9 W/(m·K)

400.0 °C

28.5 W/(m·K)

Show Material materials with Thermal conductivity of 28.5 W/(m·K)

500.0 °C

27.7 W/(m·K)

Show Material materials with Thermal conductivity of 27.7 W/(m·K)

600.0 °C

26.8 W/(m·K)

Show Material materials with Thermal conductivity of 26.8 W/(m·K)

Unlock all property charts

Thermal diffusivity

20.0 °C

7.1 mm²/s

Show Material materials with Thermal diffusivity of 7.1 mm²/s

100.0 °C

7.1 mm²/s

Show Material materials with Thermal diffusivity of 7.1 mm²/s

200.0 °C

6.9 mm²/s

Show Material materials with Thermal diffusivity of 6.9 mm²/s

300.0 °C

6.6 mm²/s

Show Material materials with Thermal diffusivity of 6.6 mm²/s

400.0 °C

6.1 mm²/s

Show Material materials with Thermal diffusivity of 6.1 mm²/s

500.0 °C

5.3 mm²/s

Show Material materials with Thermal diffusivity of 5.3 mm²/s

600.0 °C

4.5 mm²/s

Show Material materials with Thermal diffusivity of 4.5 mm²/s

Unlock all property charts

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

4.05E-7 Ω·m

Show Material materials with Electrical resistivity of 4.05E-7 Ω·m

100.0 °C

4.67E-7 Ω·m

Show Material materials with Electrical resistivity of 4.67E-7 Ω·m

200.0 °C

5.53E-7 Ω·m

Show Material materials with Electrical resistivity of 5.53E-7 Ω·m

300.0 °C

6.5E-7 Ω·m

Show Material materials with Electrical resistivity of 6.5E-7 Ω·m

400.0 °C

7.62E-7 Ω·m

Show Material materials with Electrical resistivity of 7.62E-7 Ω·m

500.0 °C

8.92E-7 Ω·m

Show Material materials with Electrical resistivity of 8.92E-7 Ω·m

600.0 °C

1.03E-6 Ω·m

Show Material materials with Electrical resistivity of 1.03E-6 Ω·m

Unlock all property charts

Chemical properties

PropertyValue

Aluminium

0.04 %

Show Material materials with Aluminium of 0.04 %

Carbon

0.17 - 0.23 %

Show Material materials with Carbon of 0.17 - 0.23 %

Chromium

3 - 3.3 %

Show Material materials with Chromium of 3 - 3.3 %

Copper

0.3 %

Show Material materials with Copper of 0.3 %

Manganese

0.3 - 0.5 %

Show Material materials with Manganese of 0.3 - 0.5 %

Molybdenum

0.5 - 0.6 %

Show Material materials with Molybdenum of 0.5 - 0.6 %

Nickel

0.3 %

Show Material materials with Nickel of 0.3 %

Phosphorus

0.03 %

Show Material materials with Phosphorus of 0.03 %

Silicon

0.15 - 0.35 %

Show Material materials with Silicon of 0.15 - 0.35 %

Sulfur

0.01 - 0.02 %

Show Material materials with Sulfur of 0.01 - 0.02 %

Vanadium

0.45 - 0.55 %

Show Material materials with Vanadium of 0.45 - 0.55 %