EN 10216-3 Grade P620QH quenched and tempered (+QT)

Want to keep this datasheet? Save it now in your required format

Description

Steel P620QH is a weldable fine-grained construction steel (alloyed high-grade steel) for pressure vessel construction. High-temperature range Application from -20 to 300 °C.

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueComment

Density

23.0 °C

7.8 g/cm³

Show Material materials with Density of 7.8 g/cm³

Typical for Steel

Mechanical

PropertyTemperatureValueComment

Elastic modulus

23.0 °C

190 - 210 GPa

Show Material materials with Elastic modulus of 190 - 210 GPa

Typical for Steel

Elongation

20.0 °C

16 %

Show Material materials with Elongation of 16 %

Elongation, transverse

20.0 °C

14 %

Show Material materials with Elongation, transverse of 14 %

Poisson's ratio

23.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

Typical for Steel

Tensile strength

20.0 °C

630 - 930 MPa

Show Material materials with Tensile strength of 630 - 930 MPa

100.0 °C

540 - 640 MPa

Show Material materials with Tensile strength of 540 - 640 MPa

150.0 °C

520 - 620 MPa

Show Material materials with Tensile strength of 520 - 620 MPa

200.0 °C

500 - 600 MPa

Show Material materials with Tensile strength of 500 - 600 MPa

250.0 °C

500 - 600 MPa

Show Material materials with Tensile strength of 500 - 600 MPa

300.0 °C

500 - 600 MPa

Show Material materials with Tensile strength of 500 - 600 MPa

Tensile strength, transverse

20.0 °C

630 - 930 MPa

Show Material materials with Tensile strength, transverse of 630 - 930 MPa

Yield strength

20.0 °C

500 - 620 MPa

Show Material materials with Yield strength of 500 - 620 MPa

Yield strength Rp0.2

100.0 °C

430 - 490 MPa

Show Material materials with Yield strength Rp0.2 of 430 - 490 MPa

150.0 °C

420 - 480 MPa

Show Material materials with Yield strength Rp0.2 of 420 - 480 MPa

200.0 °C

410 - 470 MPa

Show Material materials with Yield strength Rp0.2 of 410 - 470 MPa

250.0 °C

400 - 460 MPa

Show Material materials with Yield strength Rp0.2 of 400 - 460 MPa

300.0 °C

390 - 450 MPa

Show Material materials with Yield strength Rp0.2 of 390 - 450 MPa

Unlock all property charts

Yield strength, transverse

20.0 °C

500 - 620 MPa

Show Material materials with Yield strength, transverse of 500 - 620 MPa

Thermal

PropertyValue

Max service temperature, long

-20 - 300 °C

Show Material materials with Max service temperature, long of -20 - 300 °C

Chemical properties

PropertyValue

Aluminium

0.02 %

Show Material materials with Aluminium of 0.02 %

Carbon

0.2 %

Show Material materials with Carbon of 0.2 %

Chromium

0.3 %

Show Material materials with Chromium of 0.3 %

Copper

0.3 %

Show Material materials with Copper of 0.3 %

Manganese

1 - 1.7 %

Show Material materials with Manganese of 1 - 1.7 %

Molybdenum

0.1 %

Show Material materials with Molybdenum of 0.1 %

Nickel

0.8 %

Show Material materials with Nickel of 0.8 %

Niobium

0.05 %

Show Material materials with Niobium of 0.05 %

Nitrogen

0.02 %

Show Material materials with Nitrogen of 0.02 %

Phosphorus

0.03 %

Show Material materials with Phosphorus of 0.03 %

Silicon

0.6 %

Show Material materials with Silicon of 0.6 %

Sulfur

0.02 %

Show Material materials with Sulfur of 0.02 %

Titanium

0.04 %

Show Material materials with Titanium of 0.04 %

Vanadium

0.2 %

Show Material materials with Vanadium of 0.2 %