EN 10216-5 Grade X6CrNiNb18-10 solution annealed (+AT)

Want to keep this datasheet? Save it now in your required format

Description

Material X6CrNiNb18-10 is comparable to X 6 CrNiNb 18 10 acc. to DIN 17440: 1985-07. Its corrosion properties are comparable to 1.4541. The steel is resistant to intercrystalline corrosion also in sensitized condition, but it shows heat-crack susceptibility under certain welding conditions. Widely applicable for welded parts in chemical apparatus engineering, in food and luxury food industry, in film and photo industry as well as for household appliances. The steel is unsuitable for mirror finishing due to its Nb-content.

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

7.93 g/cm³

Show Material materials with Density of 7.93 g/cm³

Mechanical

PropertyTemperatureValue

Elastic modulus

-100.0 °C

206 GPa

Show Material materials with Elastic modulus of 206 GPa

20.0 °C

196 - 199.26 GPa

Show Material materials with Elastic modulus of 196 - 199.26 GPa

95.0 °C

194.43 GPa

Show Material materials with Elastic modulus of 194.43 GPa

100.0 °C

190 GPa

Show Material materials with Elastic modulus of 190 GPa

150.0 °C

189.61 GPa

Show Material materials with Elastic modulus of 189.61 GPa

200.0 °C

182 GPa

Show Material materials with Elastic modulus of 182 GPa

205.0 °C

184.78 GPa

Show Material materials with Elastic modulus of 184.78 GPa

260.0 °C

179.95 GPa

Show Material materials with Elastic modulus of 179.95 GPa

300.0 °C

174 GPa

Show Material materials with Elastic modulus of 174 GPa

315.0 °C

175.13 GPa

Show Material materials with Elastic modulus of 175.13 GPa

370.0 °C

170.99 GPa

Show Material materials with Elastic modulus of 170.99 GPa

400.0 °C

166 GPa

Show Material materials with Elastic modulus of 166 GPa

425.0 °C

166.16 GPa

Show Material materials with Elastic modulus of 166.16 GPa

485.0 °C

161.34 GPa

Show Material materials with Elastic modulus of 161.34 GPa

500.0 °C

158 GPa

Show Material materials with Elastic modulus of 158 GPa

540.0 °C

157.2 GPa

Show Material materials with Elastic modulus of 157.2 GPa

595.0 °C

151.69 GPa

Show Material materials with Elastic modulus of 151.69 GPa

600.0 °C

150 GPa

Show Material materials with Elastic modulus of 150 GPa

650.0 °C

147.54 GPa

Show Material materials with Elastic modulus of 147.54 GPa

700.0 °C

142 GPa

Show Material materials with Elastic modulus of 142 GPa

705.0 °C

142.72 GPa

Show Material materials with Elastic modulus of 142.72 GPa

760.0 °C

137.9 GPa

Show Material materials with Elastic modulus of 137.9 GPa

800.0 °C

134 GPa

Show Material materials with Elastic modulus of 134 GPa

815.0 °C

133.76 GPa

Show Material materials with Elastic modulus of 133.76 GPa

870.0 °C

128.93 GPa

Show Material materials with Elastic modulus of 128.93 GPa

900.0 °C

127 GPa

Show Material materials with Elastic modulus of 127 GPa

1000.0 °C

120 GPa

Show Material materials with Elastic modulus of 120 GPa

Elongation

20.0 °C

35 %

Show Material materials with Elongation of 35 %

Elongation, transverse

20.0 °C

30 %

Show Material materials with Elongation, transverse of 30 %

Poisson's ratio

20.0 °C

0.27 [-]

Show Material materials with Poisson's ratio of 0.27 [-]

95.0 °C

0.28 [-]

Show Material materials with Poisson's ratio of 0.28 [-]

150.0 °C

0.29 [-]

Show Material materials with Poisson's ratio of 0.29 [-]

205.0 °C

0.29 [-]

Show Material materials with Poisson's ratio of 0.29 [-]

260.0 °C

0.29 [-]

Show Material materials with Poisson's ratio of 0.29 [-]

315.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

370.0 °C

0.31 [-]

Show Material materials with Poisson's ratio of 0.31 [-]

425.0 °C

0.31 [-]

Show Material materials with Poisson's ratio of 0.31 [-]

485.0 °C

0.32 [-]

Show Material materials with Poisson's ratio of 0.32 [-]

540.0 °C

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

595.0 °C

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

650.0 °C

0.32 [-]

Show Material materials with Poisson's ratio of 0.32 [-]

705.0 °C

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

760.0 °C

0.35 [-]

Show Material materials with Poisson's ratio of 0.35 [-]

815.0 °C

0.35 [-]

Show Material materials with Poisson's ratio of 0.35 [-]

870.0 °C

0.36 [-]

Show Material materials with Poisson's ratio of 0.36 [-]

Unlock all property charts

Shear modulus

20.0 °C

78.6 GPa

Show Material materials with Shear modulus of 78.6 GPa

95.0 °C

75.84 GPa

Show Material materials with Shear modulus of 75.84 GPa

150.0 °C

73.77 GPa

Show Material materials with Shear modulus of 73.77 GPa

205.0 °C

71.71 GPa

Show Material materials with Shear modulus of 71.71 GPa

260.0 °C

69.64 GPa

Show Material materials with Shear modulus of 69.64 GPa

315.0 °C

67.57 GPa

Show Material materials with Shear modulus of 67.57 GPa

370.0 °C

65.5 GPa

Show Material materials with Shear modulus of 65.5 GPa

425.0 °C

63.43 GPa

Show Material materials with Shear modulus of 63.43 GPa

485.0 °C

61.36 GPa

Show Material materials with Shear modulus of 61.36 GPa

540.0 °C

59.3 GPa

Show Material materials with Shear modulus of 59.3 GPa

595.0 °C

57.23 GPa

Show Material materials with Shear modulus of 57.23 GPa

650.0 °C

55.85 GPa

Show Material materials with Shear modulus of 55.85 GPa

705.0 °C

53.78 GPa

Show Material materials with Shear modulus of 53.78 GPa

760.0 °C

51.11 GPa

Show Material materials with Shear modulus of 51.11 GPa

815.0 °C

49.64 GPa

Show Material materials with Shear modulus of 49.64 GPa

870.0 °C

47.57 GPa

Show Material materials with Shear modulus of 47.57 GPa

Unlock all property charts

Tensile strength

20.0 °C

510 - 740 MPa

Show Material materials with Tensile strength of 510 - 740 MPa

Tensile strength, transverse

20.0 °C

510 - 740 MPa

Show Material materials with Tensile strength, transverse of 510 - 740 MPa

Yield strength Rp0.2

20.0 °C

205 MPa

Show Material materials with Yield strength Rp0.2 of 205 MPa

50.0 °C

195 MPa

Show Material materials with Yield strength Rp0.2 of 195 MPa

100.0 °C

175 MPa

Show Material materials with Yield strength Rp0.2 of 175 MPa

150.0 °C

165 MPa

Show Material materials with Yield strength Rp0.2 of 165 MPa

200.0 °C

155 MPa

Show Material materials with Yield strength Rp0.2 of 155 MPa

250.0 °C

145 MPa

Show Material materials with Yield strength Rp0.2 of 145 MPa

300.0 °C

136 MPa

Show Material materials with Yield strength Rp0.2 of 136 MPa

350.0 °C

130 MPa

Show Material materials with Yield strength Rp0.2 of 130 MPa

400.0 °C

125 MPa

Show Material materials with Yield strength Rp0.2 of 125 MPa

450.0 °C

121 MPa

Show Material materials with Yield strength Rp0.2 of 121 MPa

500.0 °C

119 MPa

Show Material materials with Yield strength Rp0.2 of 119 MPa

550.0 °C

118 MPa

Show Material materials with Yield strength Rp0.2 of 118 MPa

Unlock all property charts

Yield strength Rp0.2, transverse

20.0 °C

205 MPa

Show Material materials with Yield strength Rp0.2, transverse of 205 MPa

Yield strength Rp1.0

20.0 °C

240 MPa

Show Material materials with Yield strength Rp1.0 of 240 MPa

50.0 °C

232 MPa

Show Material materials with Yield strength Rp1.0 of 232 MPa

100.0 °C

210 MPa

Show Material materials with Yield strength Rp1.0 of 210 MPa

150.0 °C

195 MPa

Show Material materials with Yield strength Rp1.0 of 195 MPa

200.0 °C

185 MPa

Show Material materials with Yield strength Rp1.0 of 185 MPa

250.0 °C

175 MPa

Show Material materials with Yield strength Rp1.0 of 175 MPa

300.0 °C

167 MPa

Show Material materials with Yield strength Rp1.0 of 167 MPa

350.0 °C

161 MPa

Show Material materials with Yield strength Rp1.0 of 161 MPa

400.0 °C

156 MPa

Show Material materials with Yield strength Rp1.0 of 156 MPa

450.0 °C

152 MPa

Show Material materials with Yield strength Rp1.0 of 152 MPa

500.0 °C

149 MPa

Show Material materials with Yield strength Rp1.0 of 149 MPa

550.0 °C

147 MPa

Show Material materials with Yield strength Rp1.0 of 147 MPa

Unlock all property charts

Yield strength Rp1.0, transverse

20.0 °C

240 MPa

Show Material materials with Yield strength Rp1.0, transverse of 240 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

-100.0 °C

1.49E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.49E-5 1/K

20.0 °C

1.61E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.61E-5 1/K

100.0 °C

1.67E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.67E-5 1/K

200.0 °C

1.72E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.72E-5 1/K

300.0 °C

1.77E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.77E-5 1/K

400.0 °C

1.81E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.81E-5 1/K

425.0 °C

1.76E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.76E-5 1/K

485.0 °C

1.78E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.78E-5 1/K

500.0 °C

1.84E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.84E-5 1/K

540.0 °C

1.8E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.8E-5 1/K

595.0 °C

1.83E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.83E-5 1/K

600.0 °C

1.88E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.88E-5 1/K

650.0 °C

1.85E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.85E-5 1/K

700.0 °C

1.91E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.91E-5 1/K

705.0 °C

1.87E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.87E-5 1/K

800.0 °C

1.94E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.94E-5 1/K

900.0 °C

1.97E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.97E-5 1/K

1000.0 °C

2E-5 1/K

Show Material materials with Coefficient of thermal expansion of 2E-5 1/K

Unlock all property charts

Melting point

1230 - 1480 °C

Show Material materials with Melting point of 1230 - 1480 °C

Typical for Austenitic Stainless Steel

Specific heat capacity

-100.0 °C

440 J/(kg·K)

Show Material materials with Specific heat capacity of 440 J/(kg·K)

20.0 °C

472 J/(kg·K)

Show Material materials with Specific heat capacity of 472 J/(kg·K)

100.0 °C

487 J/(kg·K)

Show Material materials with Specific heat capacity of 487 J/(kg·K)

200.0 °C

503 J/(kg·K)

Show Material materials with Specific heat capacity of 503 J/(kg·K)

300.0 °C

512 J/(kg·K)

Show Material materials with Specific heat capacity of 512 J/(kg·K)

400.0 °C

520 J/(kg·K)

Show Material materials with Specific heat capacity of 520 J/(kg·K)

500.0 °C

530 J/(kg·K)

Show Material materials with Specific heat capacity of 530 J/(kg·K)

600.0 °C

541 J/(kg·K)

Show Material materials with Specific heat capacity of 541 J/(kg·K)

700.0 °C

551 J/(kg·K)

Show Material materials with Specific heat capacity of 551 J/(kg·K)

800.0 °C

559 J/(kg·K)

Show Material materials with Specific heat capacity of 559 J/(kg·K)

900.0 °C

565 J/(kg·K)

Show Material materials with Specific heat capacity of 565 J/(kg·K)

1000.0 °C

571 J/(kg·K)

Show Material materials with Specific heat capacity of 571 J/(kg·K)

Unlock all property charts

Thermal conductivity

20.0 °C

14.3 W/(m·K)

Show Material materials with Thermal conductivity of 14.3 W/(m·K)

100.0 °C

15.8 W/(m·K)

Show Material materials with Thermal conductivity of 15.8 W/(m·K)

200.0 °C

17.5 W/(m·K)

Show Material materials with Thermal conductivity of 17.5 W/(m·K)

300.0 °C

19 W/(m·K)

Show Material materials with Thermal conductivity of 19 W/(m·K)

400.0 °C

20.5 W/(m·K)

Show Material materials with Thermal conductivity of 20.5 W/(m·K)

500.0 °C

21.9 W/(m·K)

Show Material materials with Thermal conductivity of 21.9 W/(m·K)

600.0 °C

23.3 W/(m·K)

Show Material materials with Thermal conductivity of 23.3 W/(m·K)

700.0 °C

24.6 W/(m·K)

Show Material materials with Thermal conductivity of 24.6 W/(m·K)

800.0 °C

26 W/(m·K)

Show Material materials with Thermal conductivity of 26 W/(m·K)

900.0 °C

27.4 W/(m·K)

Show Material materials with Thermal conductivity of 27.4 W/(m·K)

1000.0 °C

28.8 W/(m·K)

Show Material materials with Thermal conductivity of 28.8 W/(m·K)

Unlock all property charts

Thermal diffusivity

20.0 °C

3.8 mm²/s

Show Material materials with Thermal diffusivity of 3.8 mm²/s

100.0 °C

4 mm²/s

Show Material materials with Thermal diffusivity of 4 mm²/s

200.0 °C

4.2 mm²/s

Show Material materials with Thermal diffusivity of 4.2 mm²/s

300.0 °C

4.6 mm²/s

Show Material materials with Thermal diffusivity of 4.6 mm²/s

400.0 °C

4.8 mm²/s

Show Material materials with Thermal diffusivity of 4.8 mm²/s

500.0 °C

4.9 mm²/s

Show Material materials with Thermal diffusivity of 4.9 mm²/s

600.0 °C

5 mm²/s

Show Material materials with Thermal diffusivity of 5 mm²/s

700.0 °C

5.3 mm²/s

Show Material materials with Thermal diffusivity of 5.3 mm²/s

800.0 °C

5.6 mm²/s

Show Material materials with Thermal diffusivity of 5.6 mm²/s

900.0 °C

5.9 mm²/s

Show Material materials with Thermal diffusivity of 5.9 mm²/s

1000.0 °C

6 mm²/s

Show Material materials with Thermal diffusivity of 6 mm²/s

Unlock all property charts

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

7.1E-7 Ω·m

Show Material materials with Electrical resistivity of 7.1E-7 Ω·m

100.0 °C

7.76E-7 Ω·m

Show Material materials with Electrical resistivity of 7.76E-7 Ω·m

200.0 °C

8.49E-7 Ω·m

Show Material materials with Electrical resistivity of 8.49E-7 Ω·m

300.0 °C

9.14E-7 Ω·m

Show Material materials with Electrical resistivity of 9.14E-7 Ω·m

400.0 °C

9.71E-7 Ω·m

Show Material materials with Electrical resistivity of 9.71E-7 Ω·m

500.0 °C

1.02E-6 Ω·m

Show Material materials with Electrical resistivity of 1.02E-6 Ω·m

600.0 °C

1.07E-6 Ω·m

Show Material materials with Electrical resistivity of 1.07E-6 Ω·m

700.0 °C

1.1E-6 Ω·m

Show Material materials with Electrical resistivity of 1.1E-6 Ω·m

800.0 °C

1.14E-6 Ω·m

Show Material materials with Electrical resistivity of 1.14E-6 Ω·m

900.0 °C

1.17E-6 Ω·m

Show Material materials with Electrical resistivity of 1.17E-6 Ω·m

1000.0 °C

1.19E-6 Ω·m

Show Material materials with Electrical resistivity of 1.19E-6 Ω·m

Unlock all property charts

Chemical properties

PropertyValue

Carbon

0.08 %

Show Material materials with Carbon of 0.08 %

Chromium

17 - 19 %

Show Material materials with Chromium of 17 - 19 %

Manganese

2 %

Show Material materials with Manganese of 2 %

Nickel

9 - 12 %

Show Material materials with Nickel of 9 - 12 %

Niobium

1 %

Show Material materials with Niobium of 1 %

Phosphorus

0.04 %

Show Material materials with Phosphorus of 0.04 %

Silicon

1 %

Show Material materials with Silicon of 1 %

Sulfur

0.015 %

Show Material materials with Sulfur of 0.015 %