EN 10216-5 Grade X3CrNiMo17-13-3 solution annealed (+AT)

Want to keep this datasheet? Save it now in your required format

Description

X3CrNiMo17-13-3 is an austenitic steel that is resistant to intercrystalline corrosion. Temperature of solution is between 1020 and 1200°C (max. temperature is a reference data) and is cooled in water or air.

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

8 g/cm³

Show Material materials with Density of 8 g/cm³

Mechanical

PropertyTemperatureValueComment

Elastic modulus

20.0 °C

200 GPa

Show Material materials with Elastic modulus of 200 GPa

100.0 °C

194 GPa

Show Material materials with Elastic modulus of 194 GPa

200.0 °C

186 GPa

Show Material materials with Elastic modulus of 186 GPa

300.0 °C

179 GPa

Show Material materials with Elastic modulus of 179 GPa

400.0 °C

172 GPa

Show Material materials with Elastic modulus of 172 GPa

500.0 °C

165 GPa

Show Material materials with Elastic modulus of 165 GPa

Elongation

20.0 °C

40 %

Show Material materials with Elongation of 40 %

Elongation, transverse

20.0 °C

30 %

Show Material materials with Elongation, transverse of 30 %

Poisson's ratio

23.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

Typical for Austenitic Stainless Steel

Shear modulus

23.0 °C

77 GPa

Show Material materials with Shear modulus of 77 GPa

Typical for Austenitic Stainless Steel

Tensile strength

20.0 °C

510 - 710 MPa

Show Material materials with Tensile strength of 510 - 710 MPa

Tensile strength, transverse

20.0 °C

510 - 710 MPa

Show Material materials with Tensile strength, transverse of 510 - 710 MPa

Yield strength Rp0.2

20.0 °C

205 MPa

Show Material materials with Yield strength Rp0.2 of 205 MPa

50.0 °C

195 MPa

Show Material materials with Yield strength Rp0.2 of 195 MPa

100.0 °C

175 MPa

Show Material materials with Yield strength Rp0.2 of 175 MPa

150.0 °C

158 MPa

Show Material materials with Yield strength Rp0.2 of 158 MPa

200.0 °C

145 MPa

Show Material materials with Yield strength Rp0.2 of 145 MPa

250.0 °C

135 MPa

Show Material materials with Yield strength Rp0.2 of 135 MPa

300.0 °C

127 MPa

Show Material materials with Yield strength Rp0.2 of 127 MPa

350.0 °C

120 MPa

Show Material materials with Yield strength Rp0.2 of 120 MPa

400.0 °C

115 MPa

Show Material materials with Yield strength Rp0.2 of 115 MPa

450.0 °C

112 MPa

Show Material materials with Yield strength Rp0.2 of 112 MPa

500.0 °C

110 MPa

Show Material materials with Yield strength Rp0.2 of 110 MPa

550.0 °C

108 MPa

Show Material materials with Yield strength Rp0.2 of 108 MPa

Unlock all property charts

Yield strength Rp0.2, transverse

20.0 °C

205 MPa

Show Material materials with Yield strength Rp0.2, transverse of 205 MPa

Yield strength Rp1.0

20.0 °C

240 MPa

Show Material materials with Yield strength Rp1.0 of 240 MPa

50.0 °C

228 MPa

Show Material materials with Yield strength Rp1.0 of 228 MPa

100.0 °C

210 MPa

Show Material materials with Yield strength Rp1.0 of 210 MPa

150.0 °C

190 MPa

Show Material materials with Yield strength Rp1.0 of 190 MPa

200.0 °C

175 MPa

Show Material materials with Yield strength Rp1.0 of 175 MPa

250.0 °C

165 MPa

Show Material materials with Yield strength Rp1.0 of 165 MPa

300.0 °C

155 MPa

Show Material materials with Yield strength Rp1.0 of 155 MPa

350.0 °C

150 MPa

Show Material materials with Yield strength Rp1.0 of 150 MPa

400.0 °C

145 MPa

Show Material materials with Yield strength Rp1.0 of 145 MPa

450.0 °C

141 MPa

Show Material materials with Yield strength Rp1.0 of 141 MPa

500.0 °C

139 MPa

Show Material materials with Yield strength Rp1.0 of 139 MPa

550.0 °C

137 MPa

Show Material materials with Yield strength Rp1.0 of 137 MPa

Unlock all property charts

Yield strength Rp1.0, transverse

20.0 °C

240 MPa

Show Material materials with Yield strength Rp1.0, transverse of 240 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

100.0 °C

1.6E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.6E-5 1/K

200.0 °C

1.65E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.65E-5 1/K

300.0 °C

1.7E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.7E-5 1/K

400.0 °C

1.75E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.75E-5 1/K

500.0 °C

1.8E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.8E-5 1/K

Unlock all property charts

Melting point

1230 - 1480 °C

Show Material materials with Melting point of 1230 - 1480 °C

Typical for Austenitic Stainless Steel

Specific heat capacity

20.0 °C

500 J/(kg·K)

Show Material materials with Specific heat capacity of 500 J/(kg·K)

Thermal conductivity

20.0 °C

15 W/(m·K)

Show Material materials with Thermal conductivity of 15 W/(m·K)

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

7.5E-7 Ω·m

Show Material materials with Electrical resistivity of 7.5E-7 Ω·m

Chemical properties

PropertyValue

Carbon

0.05 %

Show Material materials with Carbon of 0.05 %

Chromium

16.5 - 18.5 %

Show Material materials with Chromium of 16.5 - 18.5 %

Manganese

2 %

Show Material materials with Manganese of 2 %

Molybdenum

2.5 - 3 %

Show Material materials with Molybdenum of 2.5 - 3 %

Nickel

10.5 - 13 %

Show Material materials with Nickel of 10.5 - 13 %

Nitrogen

0.11 %

Show Material materials with Nitrogen of 0.11 %

Phosphorus

0.04 %

Show Material materials with Phosphorus of 0.04 %

Silicon

1 %

Show Material materials with Silicon of 1 %

Sulfur

0.015 %

Show Material materials with Sulfur of 0.015 %