The highly corrosion resistant austenitic material X1NiCrMoCu31-27-4, mat. number 1.4563, is comparable to X 1 NiCrMoCu 31 27 4 acc. to SEW 400 : 1991-02 (invalid, replaced by edition SEW 400 : 1997-02 where this trademark is not contained anymore). The rolled and forged steel is applicable acc. to VdTÜV-material specification 483 : 1996-06 for pressure vessels acc. to TRB 100 and AD-data sheet W 2 and W 10 from -196 to 550 deg., for steam boilers as per TRD 101, TRD 102 and TRD 107 up to 550 deg. as well as for pressure gas vessels acc. TRG 201 and TRG 203 from -196 to 550 deg. Further application in nuclear power engineering as far as nuclear regulations or object-related specifications permit use from -196 to 550 deg. The material is resistant to intercrystalline corrosion up to 400 deg. both in delivery and welded condition. It shows very good resistance to stress corrosion, pitting and crevice corrosion in chloride containing media as well as good resistance to organic and inorganic acids. This material is cold and warm formable. It is within the examined dimensional range fusion weldable by metal arc welding with covered rod electrodes and TIG-welding. Preheating and heat treatment are for material reasosns not necessary. The intermediate temperature should not exceed 150 deg. for thicknesses to be welded of up to 30 mm and 100 deg. for higher thicknesses. Related or higher alloyed welding additions should be preferred with regard to the special corrosion properties of the material (e.g. welding additions acc. to VdTÜV-Wbl 1153).

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

8 - 8.08 g/cm³

Show Material materials with Density of 8 - 8.08 g/cm³

Mechanical

PropertyTemperatureValueComment

Elastic modulus

20.0 °C

191 - 195 GPa

Show Material materials with Elastic modulus of 191 - 195 GPa

100.0 °C

186 - 190 GPa

Show Material materials with Elastic modulus of 186 - 190 GPa

200.0 °C

179 - 182 GPa

Show Material materials with Elastic modulus of 179 - 182 GPa

300.0 °C

172 - 174 GPa

Show Material materials with Elastic modulus of 172 - 174 GPa

400.0 °C

166 GPa

Show Material materials with Elastic modulus of 166 GPa

500.0 °C

158 - 159 GPa

Show Material materials with Elastic modulus of 158 - 159 GPa

Elongation

20.0 °C

40 %

Show Material materials with Elongation of 40 %

Elongation, transverse

20.0 °C

35 %

Show Material materials with Elongation, transverse of 35 %

Poisson's ratio

23.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

Typical for Austenitic Stainless Steel

Shear modulus

23.0 °C

77 GPa

Show Material materials with Shear modulus of 77 GPa

Typical for Austenitic Stainless Steel

Tensile strength

20.0 °C

500 - 750 MPa

Show Material materials with Tensile strength of 500 - 750 MPa

Tensile strength, transverse

20.0 °C

500 - 750 MPa

Show Material materials with Tensile strength, transverse of 500 - 750 MPa

Yield strength Rp0.2

20.0 °C

215 MPa

Show Material materials with Yield strength Rp0.2 of 215 MPa

50.0 °C

210 MPa

Show Material materials with Yield strength Rp0.2 of 210 MPa

100.0 °C

190 MPa

Show Material materials with Yield strength Rp0.2 of 190 MPa

150.0 °C

175 MPa

Show Material materials with Yield strength Rp0.2 of 175 MPa

200.0 °C

160 MPa

Show Material materials with Yield strength Rp0.2 of 160 MPa

250.0 °C

155 MPa

Show Material materials with Yield strength Rp0.2 of 155 MPa

300.0 °C

150 MPa

Show Material materials with Yield strength Rp0.2 of 150 MPa

350.0 °C

145 MPa

Show Material materials with Yield strength Rp0.2 of 145 MPa

400.0 °C

135 MPa

Show Material materials with Yield strength Rp0.2 of 135 MPa

450.0 °C

125 MPa

Show Material materials with Yield strength Rp0.2 of 125 MPa

500.0 °C

120 MPa

Show Material materials with Yield strength Rp0.2 of 120 MPa

550.0 °C

115 MPa

Show Material materials with Yield strength Rp0.2 of 115 MPa

Unlock all property charts

Yield strength Rp0.2, transverse

20.0 °C

215 MPa

Show Material materials with Yield strength Rp0.2, transverse of 215 MPa

Yield strength Rp1.0

20.0 °C

245 MPa

Show Material materials with Yield strength Rp1.0 of 245 MPa

50.0 °C

240 MPa

Show Material materials with Yield strength Rp1.0 of 240 MPa

100.0 °C

220 MPa

Show Material materials with Yield strength Rp1.0 of 220 MPa

150.0 °C

205 MPa

Show Material materials with Yield strength Rp1.0 of 205 MPa

200.0 °C

190 MPa

Show Material materials with Yield strength Rp1.0 of 190 MPa

250.0 °C

185 MPa

Show Material materials with Yield strength Rp1.0 of 185 MPa

300.0 °C

180 MPa

Show Material materials with Yield strength Rp1.0 of 180 MPa

350.0 °C

175 MPa

Show Material materials with Yield strength Rp1.0 of 175 MPa

400.0 °C

165 MPa

Show Material materials with Yield strength Rp1.0 of 165 MPa

450.0 °C

155 MPa

Show Material materials with Yield strength Rp1.0 of 155 MPa

500.0 °C

150 MPa

Show Material materials with Yield strength Rp1.0 of 150 MPa

550.0 °C

146 MPa

Show Material materials with Yield strength Rp1.0 of 146 MPa

Unlock all property charts

Yield strength Rp1.0, transverse

20.0 °C

245 MPa

Show Material materials with Yield strength Rp1.0, transverse of 245 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

100.0 °C

1.51E-5 - 1.58E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.51E-5 - 1.58E-5 1/K

200.0 °C

1.55E-5 - 1.61E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.55E-5 - 1.61E-5 1/K

300.0 °C

1.58E-5 - 1.65E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.58E-5 - 1.65E-5 1/K

400.0 °C

1.62E-5 - 1.69E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.62E-5 - 1.69E-5 1/K

500.0 °C

1.66E-5 - 1.73E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.66E-5 - 1.73E-5 1/K

Unlock all property charts

Melting point

1230 - 1480 °C

Show Material materials with Melting point of 1230 - 1480 °C

Typical for Austenitic Stainless Steel

Specific heat capacity

20.0 °C

450 - 452 J/(kg·K)

Show Material materials with Specific heat capacity of 450 - 452 J/(kg·K)

100.0 °C

463 J/(kg·K)

Show Material materials with Specific heat capacity of 463 J/(kg·K)

200.0 °C

474 J/(kg·K)

Show Material materials with Specific heat capacity of 474 J/(kg·K)

300.0 °C

483 J/(kg·K)

Show Material materials with Specific heat capacity of 483 J/(kg·K)

400.0 °C

491 J/(kg·K)

Show Material materials with Specific heat capacity of 491 J/(kg·K)

500.0 °C

500 J/(kg·K)

Show Material materials with Specific heat capacity of 500 J/(kg·K)

Unlock all property charts

Thermal conductivity

20.0 °C

11.7 - 12 W/(m·K)

Show Material materials with Thermal conductivity of 11.7 - 12 W/(m·K)

100.0 °C

13.2 W/(m·K)

Show Material materials with Thermal conductivity of 13.2 W/(m·K)

200.0 °C

15 W/(m·K)

Show Material materials with Thermal conductivity of 15 W/(m·K)

300.0 °C

16.8 W/(m·K)

Show Material materials with Thermal conductivity of 16.8 W/(m·K)

400.0 °C

18.5 W/(m·K)

Show Material materials with Thermal conductivity of 18.5 W/(m·K)

500.0 °C

20.2 W/(m·K)

Show Material materials with Thermal conductivity of 20.2 W/(m·K)

Unlock all property charts

Thermal diffusivity

20.0 °C

3.2 mm²/s

Show Material materials with Thermal diffusivity of 3.2 mm²/s

100.0 °C

3.5 mm²/s

Show Material materials with Thermal diffusivity of 3.5 mm²/s

200.0 °C

3.8 mm²/s

Show Material materials with Thermal diffusivity of 3.8 mm²/s

300.0 °C

4.1 mm²/s

Show Material materials with Thermal diffusivity of 4.1 mm²/s

400.0 °C

4.5 mm²/s

Show Material materials with Thermal diffusivity of 4.5 mm²/s

500.0 °C

4.8 mm²/s

Show Material materials with Thermal diffusivity of 4.8 mm²/s

Unlock all property charts

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

1E-6 - 1.04E-6 Ω·m

Show Material materials with Electrical resistivity of 1E-6 - 1.04E-6 Ω·m

100.0 °C

1.07E-6 Ω·m

Show Material materials with Electrical resistivity of 1.07E-6 Ω·m

200.0 °C

1.1E-6 Ω·m

Show Material materials with Electrical resistivity of 1.1E-6 Ω·m

300.0 °C

1.13E-6 Ω·m

Show Material materials with Electrical resistivity of 1.13E-6 Ω·m

400.0 °C

1.16E-6 Ω·m

Show Material materials with Electrical resistivity of 1.16E-6 Ω·m

500.0 °C

1.18E-6 Ω·m

Show Material materials with Electrical resistivity of 1.18E-6 Ω·m

Unlock all property charts

Chemical properties

PropertyValue

Carbon

0.02 %

Show Material materials with Carbon of 0.02 %

Chromium

26 - 28 %

Show Material materials with Chromium of 26 - 28 %

Copper

0.7 - 1.5 %

Show Material materials with Copper of 0.7 - 1.5 %

Manganese

2 %

Show Material materials with Manganese of 2 %

Molybdenum

3 - 4 %

Show Material materials with Molybdenum of 3 - 4 %

Nickel

30 - 32 %

Show Material materials with Nickel of 30 - 32 %

Nitrogen

0.11 %

Show Material materials with Nitrogen of 0.11 %

Phosphorus

0.03 %

Show Material materials with Phosphorus of 0.03 %

Silicon

0.7 %

Show Material materials with Silicon of 0.7 %

Sulfur

0.01 %

Show Material materials with Sulfur of 0.01 %