EN 10216-5 Grade X1NiCrMoCu25-20-5 solution annealed (+AT)

Want to keep this datasheet? Save it now in your required format

Description

Material X 1 NiCrMoCu 25 20 5 (X1NiCrMoCu25-20-5), material number 1.4539 is applicated for pressure vessels acc. to TRB 100 and AD-data sheet W 2 and W 10 from -60 to 400 deg., for steam boilers acc. to TRD 101, TRD 102 and TRD 107 up to 400 deg. as well as for pressure gas tanks as per TRG from -60 to 400 deg. Further application in nuclear power engineering as far as nuclear regulations or object-related specifications permit use from -60 to 400 deg. The welding suitability is examined allowing for generally accepted engineering rules for arc welding, TIG-welding, submerged and plasma welding. Preheating is not necessary, intermediate temperature should not exceed 100 deg. Heat treatment after welding is only in special cases (particular corrosion load) necessary (solution annealing and quenching). This material is cold and warm formable and resistant to intercrystalline corrosion in delivery and welded condition without heat treatment up to 400 deg. To the material acc. to DIN EN 10088-1 : 1995-08 applies: Trademark X1NiCrMoCu25-20-5 is comparable to X 1 NiCrMoCuN 25 20 5 acc. to SEW 400 : 1991-02. It is an austenitic steel with high resistance to strongly attacking organic and inorganic acids, with high resistance to pitting corrosion and wide resistance to stress corrosion. It shows the second best pitting index of all steels after 1.4529 (functional sum 39). The material is resistant to intercrystalline corrosion also in welded condition. Application in chemical and petrochemical industry, for flue gas desulfurizing plants, in cellulose and paper industry as well as for smokestack linings.

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

7.76 - 8 g/cm³

Show Material materials with Density of 7.76 - 8 g/cm³

Mechanical

PropertyTemperatureValueComment

Elastic modulus

-100.0 °C

206 GPa

Show Material materials with Elastic modulus of 206 GPa

20.0 °C

195 - 196 GPa

Show Material materials with Elastic modulus of 195 - 196 GPa

100.0 °C

190 GPa

Show Material materials with Elastic modulus of 190 GPa

200.0 °C

182 GPa

Show Material materials with Elastic modulus of 182 GPa

300.0 °C

174 GPa

Show Material materials with Elastic modulus of 174 GPa

400.0 °C

166 GPa

Show Material materials with Elastic modulus of 166 GPa

500.0 °C

158 GPa

Show Material materials with Elastic modulus of 158 GPa

600.0 °C

150 GPa

Show Material materials with Elastic modulus of 150 GPa

700.0 °C

142 GPa

Show Material materials with Elastic modulus of 142 GPa

800.0 °C

134 GPa

Show Material materials with Elastic modulus of 134 GPa

900.0 °C

127 GPa

Show Material materials with Elastic modulus of 127 GPa

1000.0 °C

120 GPa

Show Material materials with Elastic modulus of 120 GPa

Elongation

20.0 °C

35 %

Show Material materials with Elongation of 35 %

Elongation, transverse

20.0 °C

30 %

Show Material materials with Elongation, transverse of 30 %

Poisson's ratio

23.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

Typical for Austenitic Stainless Steel

Shear modulus

23.0 °C

77 GPa

Show Material materials with Shear modulus of 77 GPa

Typical for Austenitic Stainless Steel

Tensile strength

20.0 °C

520 - 720 MPa

Show Material materials with Tensile strength of 520 - 720 MPa

Tensile strength, transverse

20.0 °C

520 - 720 MPa

Show Material materials with Tensile strength, transverse of 520 - 720 MPa

Yield strength Rp0.2

20.0 °C

230 MPa

Show Material materials with Yield strength Rp0.2 of 230 MPa

50.0 °C

221 MPa

Show Material materials with Yield strength Rp0.2 of 221 MPa

100.0 °C

205 MPa

Show Material materials with Yield strength Rp0.2 of 205 MPa

150.0 °C

190 MPa

Show Material materials with Yield strength Rp0.2 of 190 MPa

200.0 °C

175 MPa

Show Material materials with Yield strength Rp0.2 of 175 MPa

250.0 °C

160 MPa

Show Material materials with Yield strength Rp0.2 of 160 MPa

300.0 °C

145 MPa

Show Material materials with Yield strength Rp0.2 of 145 MPa

350.0 °C

135 MPa

Show Material materials with Yield strength Rp0.2 of 135 MPa

400.0 °C

125 MPa

Show Material materials with Yield strength Rp0.2 of 125 MPa

450.0 °C

115 MPa

Show Material materials with Yield strength Rp0.2 of 115 MPa

500.0 °C

110 MPa

Show Material materials with Yield strength Rp0.2 of 110 MPa

550.0 °C

105 MPa

Show Material materials with Yield strength Rp0.2 of 105 MPa

Unlock all property charts

Yield strength Rp0.2, transverse

20.0 °C

230 MPa

Show Material materials with Yield strength Rp0.2, transverse of 230 MPa

Yield strength Rp1.0

20.0 °C

250 MPa

Show Material materials with Yield strength Rp1.0 of 250 MPa

50.0 °C

244 MPa

Show Material materials with Yield strength Rp1.0 of 244 MPa

100.0 °C

235 MPa

Show Material materials with Yield strength Rp1.0 of 235 MPa

150.0 °C

220 MPa

Show Material materials with Yield strength Rp1.0 of 220 MPa

200.0 °C

205 MPa

Show Material materials with Yield strength Rp1.0 of 205 MPa

250.0 °C

190 MPa

Show Material materials with Yield strength Rp1.0 of 190 MPa

300.0 °C

175 MPa

Show Material materials with Yield strength Rp1.0 of 175 MPa

350.0 °C

165 MPa

Show Material materials with Yield strength Rp1.0 of 165 MPa

400.0 °C

155 MPa

Show Material materials with Yield strength Rp1.0 of 155 MPa

450.0 °C

145 MPa

Show Material materials with Yield strength Rp1.0 of 145 MPa

500.0 °C

140 MPa

Show Material materials with Yield strength Rp1.0 of 140 MPa

550.0 °C

135 MPa

Show Material materials with Yield strength Rp1.0 of 135 MPa

Unlock all property charts

Yield strength Rp1.0, transverse

20.0 °C

250 MPa

Show Material materials with Yield strength Rp1.0, transverse of 250 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

-100.0 °C

1.49E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.49E-5 1/K

20.0 °C

1.61E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.61E-5 1/K

100.0 °C

1.58E-5 - 1.67E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.58E-5 - 1.67E-5 1/K

200.0 °C

1.61E-5 - 1.72E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.61E-5 - 1.72E-5 1/K

300.0 °C

1.65E-5 - 1.77E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.65E-5 - 1.77E-5 1/K

400.0 °C

1.69E-5 - 1.81E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.69E-5 - 1.81E-5 1/K

500.0 °C

1.73E-5 - 1.84E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.73E-5 - 1.84E-5 1/K

600.0 °C

1.88E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.88E-5 1/K

700.0 °C

1.91E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.91E-5 1/K

800.0 °C

1.94E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.94E-5 1/K

900.0 °C

1.97E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.97E-5 1/K

1000.0 °C

2E-5 1/K

Show Material materials with Coefficient of thermal expansion of 2E-5 1/K

Unlock all property charts

Melting point

1230 - 1480 °C

Show Material materials with Melting point of 1230 - 1480 °C

Typical for Austenitic Stainless Steel

Specific heat capacity

-100.0 °C

440 J/(kg·K)

Show Material materials with Specific heat capacity of 440 J/(kg·K)

20.0 °C

450 - 472 J/(kg·K)

Show Material materials with Specific heat capacity of 450 - 472 J/(kg·K)

100.0 °C

487 J/(kg·K)

Show Material materials with Specific heat capacity of 487 J/(kg·K)

200.0 °C

503 J/(kg·K)

Show Material materials with Specific heat capacity of 503 J/(kg·K)

300.0 °C

512 J/(kg·K)

Show Material materials with Specific heat capacity of 512 J/(kg·K)

400.0 °C

520 J/(kg·K)

Show Material materials with Specific heat capacity of 520 J/(kg·K)

500.0 °C

530 J/(kg·K)

Show Material materials with Specific heat capacity of 530 J/(kg·K)

600.0 °C

541 J/(kg·K)

Show Material materials with Specific heat capacity of 541 J/(kg·K)

700.0 °C

551 J/(kg·K)

Show Material materials with Specific heat capacity of 551 J/(kg·K)

800.0 °C

559 J/(kg·K)

Show Material materials with Specific heat capacity of 559 J/(kg·K)

900.0 °C

565 J/(kg·K)

Show Material materials with Specific heat capacity of 565 J/(kg·K)

1000.0 °C

571 J/(kg·K)

Show Material materials with Specific heat capacity of 571 J/(kg·K)

Unlock all property charts

Thermal conductivity

20.0 °C

11.9 - 12 W/(m·K)

Show Material materials with Thermal conductivity of 11.9 - 12 W/(m·K)

100.0 °C

13.3 W/(m·K)

Show Material materials with Thermal conductivity of 13.3 W/(m·K)

200.0 °C

15.1 W/(m·K)

Show Material materials with Thermal conductivity of 15.1 W/(m·K)

300.0 °C

16.7 W/(m·K)

Show Material materials with Thermal conductivity of 16.7 W/(m·K)

400.0 °C

18.3 W/(m·K)

Show Material materials with Thermal conductivity of 18.3 W/(m·K)

500.0 °C

19.8 W/(m·K)

Show Material materials with Thermal conductivity of 19.8 W/(m·K)

600.0 °C

21.3 W/(m·K)

Show Material materials with Thermal conductivity of 21.3 W/(m·K)

700.0 °C

22.8 W/(m·K)

Show Material materials with Thermal conductivity of 22.8 W/(m·K)

800.0 °C

24.3 W/(m·K)

Show Material materials with Thermal conductivity of 24.3 W/(m·K)

900.0 °C

25.7 W/(m·K)

Show Material materials with Thermal conductivity of 25.7 W/(m·K)

1000.0 °C

27.1 W/(m·K)

Show Material materials with Thermal conductivity of 27.1 W/(m·K)

Unlock all property charts

Thermal diffusivity

20.0 °C

3.3 mm²/s

Show Material materials with Thermal diffusivity of 3.3 mm²/s

100.0 °C

3.4 mm²/s

Show Material materials with Thermal diffusivity of 3.4 mm²/s

200.0 °C

3.7 mm²/s

Show Material materials with Thermal diffusivity of 3.7 mm²/s

300.0 °C

4.1 mm²/s

Show Material materials with Thermal diffusivity of 4.1 mm²/s

400.0 °C

4.3 mm²/s

Show Material materials with Thermal diffusivity of 4.3 mm²/s

500.0 °C

4.5 mm²/s

Show Material materials with Thermal diffusivity of 4.5 mm²/s

600.0 °C

4.7 mm²/s

Show Material materials with Thermal diffusivity of 4.7 mm²/s

700.0 °C

5 mm²/s

Show Material materials with Thermal diffusivity of 5 mm²/s

800.0 °C

5.4 mm²/s

Show Material materials with Thermal diffusivity of 5.4 mm²/s

900.0 °C

5.7 mm²/s

Show Material materials with Thermal diffusivity of 5.7 mm²/s

1000.0 °C

5.8 mm²/s

Show Material materials with Thermal diffusivity of 5.8 mm²/s

Unlock all property charts

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

9.59E-7 - 1E-6 Ω·m

Show Material materials with Electrical resistivity of 9.59E-7 - 1E-6 Ω·m

100.0 °C

1.01E-6 Ω·m

Show Material materials with Electrical resistivity of 1.01E-6 Ω·m

200.0 °C

1.05E-6 Ω·m

Show Material materials with Electrical resistivity of 1.05E-6 Ω·m

300.0 °C

1.1E-6 Ω·m

Show Material materials with Electrical resistivity of 1.1E-6 Ω·m

400.0 °C

1.13E-6 Ω·m

Show Material materials with Electrical resistivity of 1.13E-6 Ω·m

500.0 °C

1.17E-6 Ω·m

Show Material materials with Electrical resistivity of 1.17E-6 Ω·m

600.0 °C

1.19E-6 Ω·m

Show Material materials with Electrical resistivity of 1.19E-6 Ω·m

700.0 °C

1.22E-6 Ω·m

Show Material materials with Electrical resistivity of 1.22E-6 Ω·m

800.0 °C

1.24E-6 Ω·m

Show Material materials with Electrical resistivity of 1.24E-6 Ω·m

900.0 °C

1.26E-6 Ω·m

Show Material materials with Electrical resistivity of 1.26E-6 Ω·m

1000.0 °C

1.28E-6 Ω·m

Show Material materials with Electrical resistivity of 1.28E-6 Ω·m

Unlock all property charts

Chemical properties

PropertyValue

Carbon

0.02 %

Show Material materials with Carbon of 0.02 %

Chromium

19 - 21 %

Show Material materials with Chromium of 19 - 21 %

Copper

1.2 - 2 %

Show Material materials with Copper of 1.2 - 2 %

Manganese

2 %

Show Material materials with Manganese of 2 %

Molybdenum

4 - 5 %

Show Material materials with Molybdenum of 4 - 5 %

Nickel

24 - 26 %

Show Material materials with Nickel of 24 - 26 %

Nitrogen

0.15 %

Show Material materials with Nitrogen of 0.15 %

Phosphorus

0.03 %

Show Material materials with Phosphorus of 0.03 %

Silicon

0.7 %

Show Material materials with Silicon of 0.7 %

Sulfur

0.01 %

Show Material materials with Sulfur of 0.01 %