EN 10216-5 Grade X1CrNiMoN25-22-2 solution annealed (+AT)

Want to keep this datasheet? Save it now in your required format

Description

Material X 2 CrNiMoN 25 22, (now: X1CrNiMoN25-22-2 ), material number 1.4466 is applicated acc. to VdT_V-Wbl 415 : 2001-09 (sheets) for pressure vessels acc. to TRB 100 and AD-data sheet W 2 and W 10 from -195 to 400 deg. (heavy duty). Further application in nuclear power engineering as far as nuclear regulations or object-related specifications permit use from -195 to 400 deg. Acc. to VdT_V-Wbl 415-2 : 2002-03 (pipes, seamless) it is used for pressure vessels as per TU 100 and AD-data sheet W 2 from -10 to 400 deg. under full loading. Further application in nuclear power engineering as far as nuclear regulations or object-related specifications permit use from -10 to 400 deg. Acc. to VdT_V-Wbl 415-3 : 2001-09 (section steel and bar steel, forged parts) it is applicable for pressure vessels as per TRB 100 and AD-data sheets W 2 and W 10 from -50 to 400 deg. Further application in nuclear power engineering as far as nuclear regulations or object-related specifications permit use from -50 to 400 deg. The welding suitability is examined allowing for generally accepted engineering rules for metal arc welding (VdT_V-Wbl 415 : 2001-09 without subsequent heat treatment), MIG-welding with covered rod electrodes, metal arc welding with welding wire and welding rods (VdT_V-Wbl 415-2 : 2002-03 preheating normally not necessary, intermediate temp. max. 200 deg., heat aftertreatment normally not necessary) and for arc hand welding resp. TIG-welding (VdT_V-Wbl 415-3 : 2001-09 preheating normally not necessary, intermediate temp. max. 150 deg., heat aftertreatment normally not necessary). To the austenitic steel X1CrNiMoN25-22-2 nach DIN EN 10088-1 : 1995-04 applies: the material is comparable to X 2 CrNiMoN 25 22 2 acc. to Key to steel 1995 resp. Register of European steels 1994. It is a fully austenitic special steel with good corrosion resistance in the urea synthesis. It is resistant to intercrystalline corrosion also in sensitized condition and polishable.

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

7.76 - 8 g/cm³

Show Material materials with Density of 7.76 - 8 g/cm³

Mechanical

PropertyTemperatureValueComment

Elastic modulus

-100.0 °C

206 GPa

Show Material materials with Elastic modulus of 206 GPa

20.0 °C

195 - 196 GPa

Show Material materials with Elastic modulus of 195 - 196 GPa

100.0 °C

190 GPa

Show Material materials with Elastic modulus of 190 GPa

200.0 °C

182 GPa

Show Material materials with Elastic modulus of 182 GPa

300.0 °C

174 GPa

Show Material materials with Elastic modulus of 174 GPa

400.0 °C

166 GPa

Show Material materials with Elastic modulus of 166 GPa

500.0 °C

158 GPa

Show Material materials with Elastic modulus of 158 GPa

600.0 °C

150 GPa

Show Material materials with Elastic modulus of 150 GPa

700.0 °C

142 GPa

Show Material materials with Elastic modulus of 142 GPa

800.0 °C

134 GPa

Show Material materials with Elastic modulus of 134 GPa

900.0 °C

127 GPa

Show Material materials with Elastic modulus of 127 GPa

1000.0 °C

120 GPa

Show Material materials with Elastic modulus of 120 GPa

Elongation

20.0 °C

40 %

Show Material materials with Elongation of 40 %

Elongation, transverse

20.0 °C

30 %

Show Material materials with Elongation, transverse of 30 %

Poisson's ratio

23.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

Typical for Austenitic Stainless Steel

Shear modulus

23.0 °C

77 GPa

Show Material materials with Shear modulus of 77 GPa

Typical for Austenitic Stainless Steel

Tensile strength

20.0 °C

540 - 740 MPa

Show Material materials with Tensile strength of 540 - 740 MPa

Tensile strength, transverse

20.0 °C

540 - 740 MPa

Show Material materials with Tensile strength, transverse of 540 - 740 MPa

Yield strength Rp0.2

20.0 °C

260 MPa

Show Material materials with Yield strength Rp0.2 of 260 MPa

50.0 °C

230 MPa

Show Material materials with Yield strength Rp0.2 of 230 MPa

100.0 °C

195 MPa

Show Material materials with Yield strength Rp0.2 of 195 MPa

150.0 °C

170 MPa

Show Material materials with Yield strength Rp0.2 of 170 MPa

200.0 °C

160 MPa

Show Material materials with Yield strength Rp0.2 of 160 MPa

250.0 °C

150 MPa

Show Material materials with Yield strength Rp0.2 of 150 MPa

300.0 °C

140 MPa

Show Material materials with Yield strength Rp0.2 of 140 MPa

350.0 °C

135 MPa

Show Material materials with Yield strength Rp0.2 of 135 MPa

Unlock all property charts

Yield strength Rp0.2, transverse

20.0 °C

260 MPa

Show Material materials with Yield strength Rp0.2, transverse of 260 MPa

Yield strength Rp1.0

20.0 °C

295 MPa

Show Material materials with Yield strength Rp1.0 of 295 MPa

50.0 °C

262 MPa

Show Material materials with Yield strength Rp1.0 of 262 MPa

100.0 °C

225 MPa

Show Material materials with Yield strength Rp1.0 of 225 MPa

150.0 °C

205 MPa

Show Material materials with Yield strength Rp1.0 of 205 MPa

200.0 °C

190 MPa

Show Material materials with Yield strength Rp1.0 of 190 MPa

250.0 °C

180 MPa

Show Material materials with Yield strength Rp1.0 of 180 MPa

300.0 °C

170 MPa

Show Material materials with Yield strength Rp1.0 of 170 MPa

350.0 °C

165 MPa

Show Material materials with Yield strength Rp1.0 of 165 MPa

Unlock all property charts

Yield strength Rp1.0, transverse

20.0 °C

295 MPa

Show Material materials with Yield strength Rp1.0, transverse of 295 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

-100.0 °C

1.49E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.49E-5 1/K

20.0 °C

1.61E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.61E-5 1/K

100.0 °C

1.57E-5 - 1.67E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.57E-5 - 1.67E-5 1/K

200.0 °C

1.72E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.72E-5 1/K

300.0 °C

1.7E-5 - 1.77E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.7E-5 - 1.77E-5 1/K

400.0 °C

1.81E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.81E-5 1/K

500.0 °C

1.84E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.84E-5 1/K

600.0 °C

1.88E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.88E-5 1/K

700.0 °C

1.91E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.91E-5 1/K

800.0 °C

1.94E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.94E-5 1/K

900.0 °C

1.97E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.97E-5 1/K

1000.0 °C

2E-5 1/K

Show Material materials with Coefficient of thermal expansion of 2E-5 1/K

Unlock all property charts

Melting point

1230 - 1480 °C

Show Material materials with Melting point of 1230 - 1480 °C

Typical for Austenitic Stainless Steel

Specific heat capacity

-100.0 °C

440 J/(kg·K)

Show Material materials with Specific heat capacity of 440 J/(kg·K)

20.0 °C

472 - 500 J/(kg·K)

Show Material materials with Specific heat capacity of 472 - 500 J/(kg·K)

100.0 °C

487 J/(kg·K)

Show Material materials with Specific heat capacity of 487 J/(kg·K)

200.0 °C

503 J/(kg·K)

Show Material materials with Specific heat capacity of 503 J/(kg·K)

300.0 °C

512 J/(kg·K)

Show Material materials with Specific heat capacity of 512 J/(kg·K)

400.0 °C

520 J/(kg·K)

Show Material materials with Specific heat capacity of 520 J/(kg·K)

500.0 °C

530 J/(kg·K)

Show Material materials with Specific heat capacity of 530 J/(kg·K)

600.0 °C

541 J/(kg·K)

Show Material materials with Specific heat capacity of 541 J/(kg·K)

700.0 °C

551 J/(kg·K)

Show Material materials with Specific heat capacity of 551 J/(kg·K)

800.0 °C

559 J/(kg·K)

Show Material materials with Specific heat capacity of 559 J/(kg·K)

900.0 °C

565 J/(kg·K)

Show Material materials with Specific heat capacity of 565 J/(kg·K)

1000.0 °C

571 J/(kg·K)

Show Material materials with Specific heat capacity of 571 J/(kg·K)

Unlock all property charts

Thermal conductivity

20.0 °C

11.9 - 14 W/(m·K)

Show Material materials with Thermal conductivity of 11.9 - 14 W/(m·K)

100.0 °C

13.3 W/(m·K)

Show Material materials with Thermal conductivity of 13.3 W/(m·K)

200.0 °C

15.1 W/(m·K)

Show Material materials with Thermal conductivity of 15.1 W/(m·K)

300.0 °C

16.7 W/(m·K)

Show Material materials with Thermal conductivity of 16.7 W/(m·K)

400.0 °C

18.3 W/(m·K)

Show Material materials with Thermal conductivity of 18.3 W/(m·K)

500.0 °C

19.8 W/(m·K)

Show Material materials with Thermal conductivity of 19.8 W/(m·K)

600.0 °C

21.3 W/(m·K)

Show Material materials with Thermal conductivity of 21.3 W/(m·K)

700.0 °C

22.8 W/(m·K)

Show Material materials with Thermal conductivity of 22.8 W/(m·K)

800.0 °C

24.3 W/(m·K)

Show Material materials with Thermal conductivity of 24.3 W/(m·K)

900.0 °C

25.7 W/(m·K)

Show Material materials with Thermal conductivity of 25.7 W/(m·K)

1000.0 °C

27.1 W/(m·K)

Show Material materials with Thermal conductivity of 27.1 W/(m·K)

Unlock all property charts

Thermal diffusivity

20.0 °C

3.3 mm²/s

Show Material materials with Thermal diffusivity of 3.3 mm²/s

100.0 °C

3.4 mm²/s

Show Material materials with Thermal diffusivity of 3.4 mm²/s

200.0 °C

3.7 mm²/s

Show Material materials with Thermal diffusivity of 3.7 mm²/s

300.0 °C

4.1 mm²/s

Show Material materials with Thermal diffusivity of 4.1 mm²/s

400.0 °C

4.3 mm²/s

Show Material materials with Thermal diffusivity of 4.3 mm²/s

500.0 °C

4.5 mm²/s

Show Material materials with Thermal diffusivity of 4.5 mm²/s

600.0 °C

4.7 mm²/s

Show Material materials with Thermal diffusivity of 4.7 mm²/s

700.0 °C

5 mm²/s

Show Material materials with Thermal diffusivity of 5 mm²/s

800.0 °C

5.4 mm²/s

Show Material materials with Thermal diffusivity of 5.4 mm²/s

900.0 °C

5.7 mm²/s

Show Material materials with Thermal diffusivity of 5.7 mm²/s

1000.0 °C

5.8 mm²/s

Show Material materials with Thermal diffusivity of 5.8 mm²/s

Unlock all property charts

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

8E-7 - 9.59E-7 Ω·m

Show Material materials with Electrical resistivity of 8E-7 - 9.59E-7 Ω·m

100.0 °C

1.01E-6 Ω·m

Show Material materials with Electrical resistivity of 1.01E-6 Ω·m

200.0 °C

1.05E-6 Ω·m

Show Material materials with Electrical resistivity of 1.05E-6 Ω·m

300.0 °C

1.1E-6 Ω·m

Show Material materials with Electrical resistivity of 1.1E-6 Ω·m

400.0 °C

1.13E-6 Ω·m

Show Material materials with Electrical resistivity of 1.13E-6 Ω·m

500.0 °C

1.17E-6 Ω·m

Show Material materials with Electrical resistivity of 1.17E-6 Ω·m

600.0 °C

1.19E-6 Ω·m

Show Material materials with Electrical resistivity of 1.19E-6 Ω·m

700.0 °C

1.22E-6 Ω·m

Show Material materials with Electrical resistivity of 1.22E-6 Ω·m

800.0 °C

1.24E-6 Ω·m

Show Material materials with Electrical resistivity of 1.24E-6 Ω·m

900.0 °C

1.26E-6 Ω·m

Show Material materials with Electrical resistivity of 1.26E-6 Ω·m

1000.0 °C

1.28E-6 Ω·m

Show Material materials with Electrical resistivity of 1.28E-6 Ω·m

Unlock all property charts

Chemical properties

PropertyValue

Carbon

0.02 %

Show Material materials with Carbon of 0.02 %

Chromium

24 - 26 %

Show Material materials with Chromium of 24 - 26 %

Manganese

2 %

Show Material materials with Manganese of 2 %

Molybdenum

2 - 2.5 %

Show Material materials with Molybdenum of 2 - 2.5 %

Nickel

21 - 23 %

Show Material materials with Nickel of 21 - 23 %

Nitrogen

0.1 - 0.16 %

Show Material materials with Nitrogen of 0.1 - 0.16 %

Phosphorus

0.03 %

Show Material materials with Phosphorus of 0.03 %

Silicon

0.7 %

Show Material materials with Silicon of 0.7 %

Sulfur

0.01 %

Show Material materials with Sulfur of 0.01 %