EN 10216-5 Grade X6CrNiMo17-13-2 solution annealed (+AT)

Want to keep this datasheet? Save it now in your required format

Description

The heat resistant steel X6CrNiMo17-13-2 (1.4918) is used for pressurised seamless tubes.

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

8 g/cm³

Show Material materials with Density of 8 g/cm³

Mechanical

PropertyTemperatureValueComment

Elastic modulus

20.0 °C

200 GPa

Show Material materials with Elastic modulus of 200 GPa

100.0 °C

194 GPa

Show Material materials with Elastic modulus of 194 GPa

200.0 °C

186 GPa

Show Material materials with Elastic modulus of 186 GPa

300.0 °C

179 GPa

Show Material materials with Elastic modulus of 179 GPa

400.0 °C

172 GPa

Show Material materials with Elastic modulus of 172 GPa

500.0 °C

165 GPa

Show Material materials with Elastic modulus of 165 GPa

600.0 °C

155 GPa

Show Material materials with Elastic modulus of 155 GPa

Elongation

20.0 °C

35 %

Show Material materials with Elongation of 35 %

Elongation, transverse

20.0 °C

30 %

Show Material materials with Elongation, transverse of 30 %

Poisson's ratio

23.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

Typical for Austenitic Stainless Steel

Shear modulus

23.0 °C

77 GPa

Show Material materials with Shear modulus of 77 GPa

Typical for Austenitic Stainless Steel

Yield strength Rp0.2

20.0 °C

205 MPa

Show Material materials with Yield strength Rp0.2 of 205 MPa

50.0 °C

184 MPa

Show Material materials with Yield strength Rp0.2 of 184 MPa

100.0 °C

177 MPa

Show Material materials with Yield strength Rp0.2 of 177 MPa

150.0 °C

162 MPa

Show Material materials with Yield strength Rp0.2 of 162 MPa

200.0 °C

147 MPa

Show Material materials with Yield strength Rp0.2 of 147 MPa

250.0 °C

137 MPa

Show Material materials with Yield strength Rp0.2 of 137 MPa

300.0 °C

127 MPa

Show Material materials with Yield strength Rp0.2 of 127 MPa

350.0 °C

122 MPa

Show Material materials with Yield strength Rp0.2 of 122 MPa

400.0 °C

118 MPa

Show Material materials with Yield strength Rp0.2 of 118 MPa

450.0 °C

113 MPa

Show Material materials with Yield strength Rp0.2 of 113 MPa

500.0 °C

108 MPa

Show Material materials with Yield strength Rp0.2 of 108 MPa

550.0 °C

103 MPa

Show Material materials with Yield strength Rp0.2 of 103 MPa

Unlock all property charts

Yield strength Rp0.2, transverse

20.0 °C

205 MPa

Show Material materials with Yield strength Rp0.2, transverse of 205 MPa

Yield strength Rp1.0

20.0 °C

245 MPa

Show Material materials with Yield strength Rp1.0 of 245 MPa

50.0 °C

228 MPa

Show Material materials with Yield strength Rp1.0 of 228 MPa

100.0 °C

211 MPa

Show Material materials with Yield strength Rp1.0 of 211 MPa

150.0 °C

194 MPa

Show Material materials with Yield strength Rp1.0 of 194 MPa

200.0 °C

177 MPa

Show Material materials with Yield strength Rp1.0 of 177 MPa

250.0 °C

167 MPa

Show Material materials with Yield strength Rp1.0 of 167 MPa

300.0 °C

157 MPa

Show Material materials with Yield strength Rp1.0 of 157 MPa

350.0 °C

152 MPa

Show Material materials with Yield strength Rp1.0 of 152 MPa

400.0 °C

147 MPa

Show Material materials with Yield strength Rp1.0 of 147 MPa

450.0 °C

142 MPa

Show Material materials with Yield strength Rp1.0 of 142 MPa

500.0 °C

137 MPa

Show Material materials with Yield strength Rp1.0 of 137 MPa

550.0 °C

132 MPa

Show Material materials with Yield strength Rp1.0 of 132 MPa

Unlock all property charts

Yield strength Rp1.0, transverse

20.0 °C

245 MPa

Show Material materials with Yield strength Rp1.0, transverse of 245 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

100.0 °C

1.6E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.6E-5 1/K

200.0 °C

1.65E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.65E-5 1/K

300.0 °C

1.7E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.7E-5 1/K

400.0 °C

1.75E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.75E-5 1/K

500.0 °C

1.8E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.8E-5 1/K

600.0 °C

1.85E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.85E-5 1/K

Unlock all property charts

Melting point

1230 - 1480 °C

Show Material materials with Melting point of 1230 - 1480 °C

Typical for Austenitic Stainless Steel

Specific heat capacity

20.0 °C

500 J/(kg·K)

Show Material materials with Specific heat capacity of 500 J/(kg·K)

Thermal conductivity

20.0 °C

15 W/(m·K)

Show Material materials with Thermal conductivity of 15 W/(m·K)

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

7.5E-7 Ω·m

Show Material materials with Electrical resistivity of 7.5E-7 Ω·m

Chemical properties

PropertyValue

Carbon

0.04 - 0.08 %

Show Material materials with Carbon of 0.04 - 0.08 %

Chromium

16 - 18 %

Show Material materials with Chromium of 16 - 18 %

Manganese

2 %

Show Material materials with Manganese of 2 %

Molybdenum

2 - 2.5 %

Show Material materials with Molybdenum of 2 - 2.5 %

Nickel

12 - 14 %

Show Material materials with Nickel of 12 - 14 %

Nitrogen

0.11 %

Show Material materials with Nitrogen of 0.11 %

Phosphorus

0.04 %

Show Material materials with Phosphorus of 0.04 %

Silicon

0.75 %

Show Material materials with Silicon of 0.75 %

Sulfur

0.015 %

Show Material materials with Sulfur of 0.015 %