EN 10216-5 Grade X10CrNiMoMnNbVB15-10-1 solution annealed (+AT)

Want to keep this datasheet? Save it now in your required format

Description

The high heat resistant steel X10CrNiMoMnNbVB15-10-1 (1.4982) is used for fasteners and for pressurised seamless tubes.

Related Standards

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

8 g/cm³

Show Material materials with Density of 8 g/cm³

Mechanical

PropertyTemperatureValueComment

Elastic modulus

20.0 °C

207 GPa

Show Material materials with Elastic modulus of 207 GPa

100.0 °C

201 GPa

Show Material materials with Elastic modulus of 201 GPa

200.0 °C

193 GPa

Show Material materials with Elastic modulus of 193 GPa

300.0 °C

184 GPa

Show Material materials with Elastic modulus of 184 GPa

400.0 °C

175 GPa

Show Material materials with Elastic modulus of 175 GPa

500.0 °C

165 GPa

Show Material materials with Elastic modulus of 165 GPa

600.0 °C

158 GPa

Show Material materials with Elastic modulus of 158 GPa

Elongation

20.0 °C

35 %

Show Material materials with Elongation of 35 %

Elongation, transverse

20.0 °C

30 %

Show Material materials with Elongation, transverse of 30 %

Poisson's ratio

23.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

Typical for Austenitic Stainless Steel

Shear modulus

23.0 °C

77 GPa

Show Material materials with Shear modulus of 77 GPa

Typical for Austenitic Stainless Steel

Yield strength Rp0.2

20.0 °C

220 MPa

Show Material materials with Yield strength Rp0.2 of 220 MPa

50.0 °C

213 MPa

Show Material materials with Yield strength Rp0.2 of 213 MPa

100.0 °C

188 MPa

Show Material materials with Yield strength Rp0.2 of 188 MPa

150.0 °C

171 MPa

Show Material materials with Yield strength Rp0.2 of 171 MPa

200.0 °C

161 MPa

Show Material materials with Yield strength Rp0.2 of 161 MPa

250.0 °C

153 MPa

Show Material materials with Yield strength Rp0.2 of 153 MPa

300.0 °C

148 MPa

Show Material materials with Yield strength Rp0.2 of 148 MPa

350.0 °C

145 MPa

Show Material materials with Yield strength Rp0.2 of 145 MPa

400.0 °C

144 MPa

Show Material materials with Yield strength Rp0.2 of 144 MPa

450.0 °C

141 MPa

Show Material materials with Yield strength Rp0.2 of 141 MPa

500.0 °C

139 MPa

Show Material materials with Yield strength Rp0.2 of 139 MPa

550.0 °C

136 MPa

Show Material materials with Yield strength Rp0.2 of 136 MPa

Unlock all property charts

Yield strength Rp0.2, transverse

20.0 °C

220 MPa

Show Material materials with Yield strength Rp0.2, transverse of 220 MPa

Yield strength Rp1.0

20.0 °C

270 MPa

Show Material materials with Yield strength Rp1.0 of 270 MPa

50.0 °C

254 MPa

Show Material materials with Yield strength Rp1.0 of 254 MPa

100.0 °C

232 MPa

Show Material materials with Yield strength Rp1.0 of 232 MPa

150.0 °C

210 MPa

Show Material materials with Yield strength Rp1.0 of 210 MPa

200.0 °C

195 MPa

Show Material materials with Yield strength Rp1.0 of 195 MPa

250.0 °C

190 MPa

Show Material materials with Yield strength Rp1.0 of 190 MPa

300.0 °C

187 MPa

Show Material materials with Yield strength Rp1.0 of 187 MPa

350.0 °C

184 MPa

Show Material materials with Yield strength Rp1.0 of 184 MPa

400.0 °C

182 MPa

Show Material materials with Yield strength Rp1.0 of 182 MPa

450.0 °C

179 MPa

Show Material materials with Yield strength Rp1.0 of 179 MPa

500.0 °C

178 MPa

Show Material materials with Yield strength Rp1.0 of 178 MPa

550.0 °C

175 MPa

Show Material materials with Yield strength Rp1.0 of 175 MPa

Unlock all property charts

Yield strength Rp1.0, transverse

20.0 °C

270 MPa

Show Material materials with Yield strength Rp1.0, transverse of 270 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

100.0 °C

1.57E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.57E-5 1/K

200.0 °C

1.68E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.68E-5 1/K

300.0 °C

1.77E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.77E-5 1/K

400.0 °C

1.83E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.83E-5 1/K

500.0 °C

1.86E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.86E-5 1/K

600.0 °C

1.9E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.9E-5 1/K

Unlock all property charts

Melting point

1230 - 1480 °C

Show Material materials with Melting point of 1230 - 1480 °C

Typical for Austenitic Stainless Steel

Specific heat capacity

20.0 °C

480 J/(kg·K)

Show Material materials with Specific heat capacity of 480 J/(kg·K)

Thermal conductivity

20.0 °C

12.5 W/(m·K)

Show Material materials with Thermal conductivity of 12.5 W/(m·K)

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

7.4E-7 Ω·m

Show Material materials with Electrical resistivity of 7.4E-7 Ω·m

Chemical properties

PropertyValue

Boron

3E-3 - 9E-3 %

Show Material materials with Boron of 3E-3 - 9E-3 %

Carbon

0.06 - 0.15 %

Show Material materials with Carbon of 0.06 - 0.15 %

Chromium

14 - 16 %

Show Material materials with Chromium of 14 - 16 %

Manganese

5.5 - 7 %

Show Material materials with Manganese of 5.5 - 7 %

Molybdenum

0.8 - 1.2 %

Show Material materials with Molybdenum of 0.8 - 1.2 %

Nickel

9 - 11 %

Show Material materials with Nickel of 9 - 11 %

Niobium

0.75 - 1.25 %

Show Material materials with Niobium of 0.75 - 1.25 %

Nitrogen

0.06 - 0.14 %

Show Material materials with Nitrogen of 0.06 - 0.14 %

Phosphorus

0.04 %

Show Material materials with Phosphorus of 0.04 %

Silicon

0.2 - 1 %

Show Material materials with Silicon of 0.2 - 1 %

Sulfur

0.015 %

Show Material materials with Sulfur of 0.015 %

Vanadium

0.15 - 0.4 %

Show Material materials with Vanadium of 0.15 - 0.4 %