EN 10217-5 Grade P265GH normalized or normalized formed (+N)

Want to keep this datasheet? Save it now in your required format

Description

Submerged-arc welded tubes made of the heat-resistant non-alloy quality steel P265GH are used for steam pressure vessels, tube construction, pressure vessel and apparatus manufacturing mainly in the chemical industry for temperatures up to 200 °C and simultaneous high pressures. The total load and the special scale relationships may decrease or increase the temperature limit.

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

7.85 g/cm³

Show Material materials with Density of 7.85 g/cm³

Mechanical

PropertyTemperatureValueComment

Elastic modulus

-100.0 °C

217 GPa

Show Material materials with Elastic modulus of 217 GPa

20.0 °C

212 GPa

Show Material materials with Elastic modulus of 212 GPa

100.0 °C

207 GPa

Show Material materials with Elastic modulus of 207 GPa

200.0 °C

199 GPa

Show Material materials with Elastic modulus of 199 GPa

300.0 °C

192 GPa

Show Material materials with Elastic modulus of 192 GPa

400.0 °C

184 GPa

Show Material materials with Elastic modulus of 184 GPa

500.0 °C

175 GPa

Show Material materials with Elastic modulus of 175 GPa

600.0 °C

164 GPa

Show Material materials with Elastic modulus of 164 GPa

Elongation

20.0 °C

23 %

Show Material materials with Elongation of 23 %

Elongation, transverse

20.0 °C

21 %

Show Material materials with Elongation, transverse of 21 %

Poisson's ratio

23.0 °C

0.29 [-]

Show Material materials with Poisson's ratio of 0.29 [-]

Typical for Low Carbon Steel

Shear modulus

23.0 °C

82 GPa

Show Material materials with Shear modulus of 82 GPa

Typical for Low Carbon Steel

Tensile strength

20.0 °C

410 - 570 MPa

Show Material materials with Tensile strength of 410 - 570 MPa

Tensile strength, transverse

20.0 °C

410 - 570 MPa

Show Material materials with Tensile strength, transverse of 410 - 570 MPa

Yield strength

20.0 °C

255 - 265 MPa

Show Material materials with Yield strength of 255 - 265 MPa

100.0 °C

228 - 238 MPa

Show Material materials with Yield strength of 228 - 238 MPa

150.0 °C

211 - 221 MPa

Show Material materials with Yield strength of 211 - 221 MPa

200.0 °C

195 - 205 MPa

Show Material materials with Yield strength of 195 - 205 MPa

250.0 °C

175 - 185 MPa

Show Material materials with Yield strength of 175 - 185 MPa

300.0 °C

155 - 160 MPa

Show Material materials with Yield strength of 155 - 160 MPa

350.0 °C

141 MPa

Show Material materials with Yield strength of 141 MPa

400.0 °C

134 MPa

Show Material materials with Yield strength of 134 MPa

450.0 °C

128 MPa

Show Material materials with Yield strength of 128 MPa

Unlock all property charts

Yield strength Rp0.2

20.0 °C

255 - 265 MPa

Show Material materials with Yield strength Rp0.2 of 255 - 265 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

-100.0 °C

1.08E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.08E-5 1/K

20.0 °C

1.19E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.19E-5 1/K

100.0 °C

1.25E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.25E-5 1/K

200.0 °C

1.3E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.3E-5 1/K

300.0 °C

1.36E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.36E-5 1/K

400.0 °C

1.41E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.41E-5 1/K

500.0 °C

1.45E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.45E-5 1/K

600.0 °C

1.49E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.49E-5 1/K

Unlock all property charts

Max service temperature

500 °C

Show Material materials with Max service temperature of 500 °C

Typical for Carbon Steel

Max service temperature, long

200 - 400 °C

Show Material materials with Max service temperature, long of 200 - 400 °C

Melting point

1480 - 1526 °C

Show Material materials with Melting point of 1480 - 1526 °C

Typical for Low Carbon Steel

Specific heat capacity

-100.0 °C

423 J/(kg·K)

Show Material materials with Specific heat capacity of 423 J/(kg·K)

20.0 °C

461 J/(kg·K)

Show Material materials with Specific heat capacity of 461 J/(kg·K)

100.0 °C

479 J/(kg·K)

Show Material materials with Specific heat capacity of 479 J/(kg·K)

200.0 °C

499 J/(kg·K)

Show Material materials with Specific heat capacity of 499 J/(kg·K)

300.0 °C

517 J/(kg·K)

Show Material materials with Specific heat capacity of 517 J/(kg·K)

400.0 °C

536 J/(kg·K)

Show Material materials with Specific heat capacity of 536 J/(kg·K)

500.0 °C

558 J/(kg·K)

Show Material materials with Specific heat capacity of 558 J/(kg·K)

600.0 °C

587 J/(kg·K)

Show Material materials with Specific heat capacity of 587 J/(kg·K)

Unlock all property charts

Thermal conductivity

20.0 °C

51 W/(m·K)

Show Material materials with Thermal conductivity of 51 W/(m·K)

100.0 °C

50.8 W/(m·K)

Show Material materials with Thermal conductivity of 50.8 W/(m·K)

200.0 °C

48.7 W/(m·K)

Show Material materials with Thermal conductivity of 48.7 W/(m·K)

300.0 °C

45.8 W/(m·K)

Show Material materials with Thermal conductivity of 45.8 W/(m·K)

400.0 °C

42.5 W/(m·K)

Show Material materials with Thermal conductivity of 42.5 W/(m·K)

500.0 °C

39.2 W/(m·K)

Show Material materials with Thermal conductivity of 39.2 W/(m·K)

600.0 °C

36 W/(m·K)

Show Material materials with Thermal conductivity of 36 W/(m·K)

Unlock all property charts

Thermal diffusivity

20.0 °C

14.1 mm²/s

Show Material materials with Thermal diffusivity of 14.1 mm²/s

100.0 °C

13.1 mm²/s

Show Material materials with Thermal diffusivity of 13.1 mm²/s

200.0 °C

11.7 mm²/s

Show Material materials with Thermal diffusivity of 11.7 mm²/s

300.0 °C

10.4 mm²/s

Show Material materials with Thermal diffusivity of 10.4 mm²/s

400.0 °C

9 mm²/s

Show Material materials with Thermal diffusivity of 9 mm²/s

500.0 °C

7.6 mm²/s

Show Material materials with Thermal diffusivity of 7.6 mm²/s

600.0 °C

6.1 mm²/s

Show Material materials with Thermal diffusivity of 6.1 mm²/s

Unlock all property charts

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

2.04E-7 Ω·m

Show Material materials with Electrical resistivity of 2.04E-7 Ω·m

100.0 °C

2.52E-7 Ω·m

Show Material materials with Electrical resistivity of 2.52E-7 Ω·m

200.0 °C

3.24E-7 Ω·m

Show Material materials with Electrical resistivity of 3.24E-7 Ω·m

300.0 °C

4.1E-7 Ω·m

Show Material materials with Electrical resistivity of 4.1E-7 Ω·m

400.0 °C

5.12E-7 Ω·m

Show Material materials with Electrical resistivity of 5.12E-7 Ω·m

500.0 °C

6.31E-7 Ω·m

Show Material materials with Electrical resistivity of 6.31E-7 Ω·m

600.0 °C

7.7E-7 Ω·m

Show Material materials with Electrical resistivity of 7.7E-7 Ω·m

Unlock all property charts

Magnetic

PropertyValueComment

Curie temperature

770 °C

Show Material materials with Curie temperature of 770 °C

Typical for Low Carbon Steel

Chemical properties

PropertyValue

Aluminium

0.02 %

Show Material materials with Aluminium of 0.02 %

Carbon

0.2 %

Show Material materials with Carbon of 0.2 %

Chromium

0.3 %

Show Material materials with Chromium of 0.3 %

Copper

0.3 %

Show Material materials with Copper of 0.3 %

Manganese

1.4 %

Show Material materials with Manganese of 1.4 %

Molybdenum

0.08 %

Show Material materials with Molybdenum of 0.08 %

Nickel

0.3 %

Show Material materials with Nickel of 0.3 %

Niobium

0.01 %

Show Material materials with Niobium of 0.01 %

Phosphorus

0.03 %

Show Material materials with Phosphorus of 0.03 %

Silicon

0.4 %

Show Material materials with Silicon of 0.4 %

Sulfur

0.02 %

Show Material materials with Sulfur of 0.02 %

Titanium

0.03 %

Show Material materials with Titanium of 0.03 %

Vanadium

0.02 %

Show Material materials with Vanadium of 0.02 %