EN 10217-7 Grade X6CrNiNb18-10 solution annealed (+AT)

View suppliers (13)
Want to keep this datasheet? Save it now in your required format

Description

The austenitic steel X6CrNiNb18-10 is available in the solution annealed condition. Welded circular tubes of this steel are used for compression load and for corrosive load at room temperature, low temperatures and elevated temperatures. The material is resistant to intercrystalline corrosion (up to 400 °C) also in the welded condition.

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

"Typical" values were obtained via a literature search. "Predicted" values were imputed via artificial intelligence technology. While we have placed significant efforts in ensuring data accuracy, "typical" and "predicted" data should be considered indicative and verified by appropriate material testing. Please do contact us if additional information on the the predicted data method is required.
All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

7.9 - 7.93 g/cm³

Show Material materials with Density of 7.9 - 7.93 g/cm³

Mechanical

PropertyTemperatureValueComment

Elastic modulus

-100.0 °C

206 GPa

Show Material materials with Elastic modulus of 206 GPa

20.0 °C

196 - 200 GPa

Show Material materials with Elastic modulus of 196 - 200 GPa

100.0 °C

190 - 194 GPa

Show Material materials with Elastic modulus of 190 - 194 GPa

200.0 °C

182 - 186 GPa

Show Material materials with Elastic modulus of 182 - 186 GPa

300.0 °C

174 - 179 GPa

Show Material materials with Elastic modulus of 174 - 179 GPa

400.0 °C

166 - 172 GPa

Show Material materials with Elastic modulus of 166 - 172 GPa

500.0 °C

158 - 165 GPa

Show Material materials with Elastic modulus of 158 - 165 GPa

600.0 °C

150 GPa

Show Material materials with Elastic modulus of 150 GPa

700.0 °C

142 GPa

Show Material materials with Elastic modulus of 142 GPa

800.0 °C

134 GPa

Show Material materials with Elastic modulus of 134 GPa

900.0 °C

127 GPa

Show Material materials with Elastic modulus of 127 GPa

1000.0 °C

120 GPa

Show Material materials with Elastic modulus of 120 GPa

Elongation

20.0 °C

35 %

Show Material materials with Elongation of 35 %

Elongation, transverse

20.0 °C

30 %

Show Material materials with Elongation, transverse of 30 %

Poisson's ratio

23.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

Typical for Austenitic Stainless Steel

Shear modulus

23.0 °C

77 GPa

Show Material materials with Shear modulus of 77 GPa

Typical for Austenitic Stainless Steel

Tensile strength

20.0 °C

510 - 740 MPa

Show Material materials with Tensile strength of 510 - 740 MPa

Tensile strength, transverse

20.0 °C

510 - 740 MPa

Show Material materials with Tensile strength, transverse of 510 - 740 MPa

Yield strength Rp0.2

20.0 °C

205 MPa

Show Material materials with Yield strength Rp0.2 of 205 MPa

50.0 °C

195 MPa

Show Material materials with Yield strength Rp0.2 of 195 MPa

100.0 °C

175 MPa

Show Material materials with Yield strength Rp0.2 of 175 MPa

150.0 °C

165 MPa

Show Material materials with Yield strength Rp0.2 of 165 MPa

200.0 °C

155 MPa

Show Material materials with Yield strength Rp0.2 of 155 MPa

250.0 °C

145 MPa

Show Material materials with Yield strength Rp0.2 of 145 MPa

300.0 °C

136 MPa

Show Material materials with Yield strength Rp0.2 of 136 MPa

350.0 °C

130 MPa

Show Material materials with Yield strength Rp0.2 of 130 MPa

400.0 °C

125 MPa

Show Material materials with Yield strength Rp0.2 of 125 MPa

450.0 °C

121 MPa

Show Material materials with Yield strength Rp0.2 of 121 MPa

500.0 °C

119 MPa

Show Material materials with Yield strength Rp0.2 of 119 MPa

550.0 °C

118 MPa

Show Material materials with Yield strength Rp0.2 of 118 MPa

Unlock all property charts

Yield strength Rp0.2, transverse

20.0 °C

205 MPa

Show Material materials with Yield strength Rp0.2, transverse of 205 MPa

Yield strength Rp1.0

20.0 °C

240 MPa

Show Material materials with Yield strength Rp1.0 of 240 MPa

50.0 °C

232 MPa

Show Material materials with Yield strength Rp1.0 of 232 MPa

100.0 °C

210 MPa

Show Material materials with Yield strength Rp1.0 of 210 MPa

150.0 °C

195 MPa

Show Material materials with Yield strength Rp1.0 of 195 MPa

200.0 °C

185 MPa

Show Material materials with Yield strength Rp1.0 of 185 MPa

250.0 °C

175 MPa

Show Material materials with Yield strength Rp1.0 of 175 MPa

300.0 °C

167 MPa

Show Material materials with Yield strength Rp1.0 of 167 MPa

350.0 °C

161 MPa

Show Material materials with Yield strength Rp1.0 of 161 MPa

400.0 °C

156 MPa

Show Material materials with Yield strength Rp1.0 of 156 MPa

450.0 °C

152 MPa

Show Material materials with Yield strength Rp1.0 of 152 MPa

500.0 °C

149 MPa

Show Material materials with Yield strength Rp1.0 of 149 MPa

550.0 °C

147 MPa

Show Material materials with Yield strength Rp1.0 of 147 MPa

Unlock all property charts

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

-100.0 °C

1.49E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.49E-5 1/K

20.0 °C

1.61E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.61E-5 1/K

100.0 °C

1.6E-5 - 1.67E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.6E-5 - 1.67E-5 1/K

200.0 °C

1.65E-5 - 1.72E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.65E-5 - 1.72E-5 1/K

300.0 °C

1.7E-5 - 1.77E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.7E-5 - 1.77E-5 1/K

400.0 °C

1.75E-5 - 1.81E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.75E-5 - 1.81E-5 1/K

500.0 °C

1.8E-5 - 1.84E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.8E-5 - 1.84E-5 1/K

600.0 °C

1.88E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.88E-5 1/K

700.0 °C

1.91E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.91E-5 1/K

800.0 °C

1.94E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.94E-5 1/K

900.0 °C

1.97E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.97E-5 1/K

1000.0 °C

2E-5 1/K

Show Material materials with Coefficient of thermal expansion of 2E-5 1/K

Unlock all property charts

Melting point

1230 - 1480 °C

Show Material materials with Melting point of 1230 - 1480 °C

Typical for Austenitic Stainless Steel

Specific heat capacity

-100.0 °C

440 J/(kg·K)

Show Material materials with Specific heat capacity of 440 J/(kg·K)

20.0 °C

472 - 500 J/(kg·K)

Show Material materials with Specific heat capacity of 472 - 500 J/(kg·K)

100.0 °C

487 J/(kg·K)

Show Material materials with Specific heat capacity of 487 J/(kg·K)

200.0 °C

503 J/(kg·K)

Show Material materials with Specific heat capacity of 503 J/(kg·K)

300.0 °C

512 J/(kg·K)

Show Material materials with Specific heat capacity of 512 J/(kg·K)

400.0 °C

520 J/(kg·K)

Show Material materials with Specific heat capacity of 520 J/(kg·K)

500.0 °C

530 J/(kg·K)

Show Material materials with Specific heat capacity of 530 J/(kg·K)

600.0 °C

541 J/(kg·K)

Show Material materials with Specific heat capacity of 541 J/(kg·K)

700.0 °C

551 J/(kg·K)

Show Material materials with Specific heat capacity of 551 J/(kg·K)

800.0 °C

559 J/(kg·K)

Show Material materials with Specific heat capacity of 559 J/(kg·K)

900.0 °C

565 J/(kg·K)

Show Material materials with Specific heat capacity of 565 J/(kg·K)

1000.0 °C

571 J/(kg·K)

Show Material materials with Specific heat capacity of 571 J/(kg·K)

Unlock all property charts

Thermal conductivity

20.0 °C

14.3 - 15 W/(m·K)

Show Material materials with Thermal conductivity of 14.3 - 15 W/(m·K)

100.0 °C

15.8 W/(m·K)

Show Material materials with Thermal conductivity of 15.8 W/(m·K)

200.0 °C

17.5 W/(m·K)

Show Material materials with Thermal conductivity of 17.5 W/(m·K)

300.0 °C

19 W/(m·K)

Show Material materials with Thermal conductivity of 19 W/(m·K)

400.0 °C

20.5 W/(m·K)

Show Material materials with Thermal conductivity of 20.5 W/(m·K)

500.0 °C

21.9 W/(m·K)

Show Material materials with Thermal conductivity of 21.9 W/(m·K)

600.0 °C

23.3 W/(m·K)

Show Material materials with Thermal conductivity of 23.3 W/(m·K)

700.0 °C

24.6 W/(m·K)

Show Material materials with Thermal conductivity of 24.6 W/(m·K)

800.0 °C

26 W/(m·K)

Show Material materials with Thermal conductivity of 26 W/(m·K)

900.0 °C

27.4 W/(m·K)

Show Material materials with Thermal conductivity of 27.4 W/(m·K)

1000.0 °C

28.8 W/(m·K)

Show Material materials with Thermal conductivity of 28.8 W/(m·K)

Unlock all property charts

Thermal diffusivity

20.0 °C

3.8 mm²/s

Show Material materials with Thermal diffusivity of 3.8 mm²/s

100.0 °C

4 mm²/s

Show Material materials with Thermal diffusivity of 4 mm²/s

200.0 °C

4.2 mm²/s

Show Material materials with Thermal diffusivity of 4.2 mm²/s

300.0 °C

4.6 mm²/s

Show Material materials with Thermal diffusivity of 4.6 mm²/s

400.0 °C

4.8 mm²/s

Show Material materials with Thermal diffusivity of 4.8 mm²/s

500.0 °C

4.9 mm²/s

Show Material materials with Thermal diffusivity of 4.9 mm²/s

600.0 °C

5 mm²/s

Show Material materials with Thermal diffusivity of 5 mm²/s

700.0 °C

5.3 mm²/s

Show Material materials with Thermal diffusivity of 5.3 mm²/s

800.0 °C

5.6 mm²/s

Show Material materials with Thermal diffusivity of 5.6 mm²/s

900.0 °C

5.9 mm²/s

Show Material materials with Thermal diffusivity of 5.9 mm²/s

1000.0 °C

6 mm²/s

Show Material materials with Thermal diffusivity of 6 mm²/s

Unlock all property charts

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

7.1E-7 - 7.3E-7 Ω·m

Show Material materials with Electrical resistivity of 7.1E-7 - 7.3E-7 Ω·m

100.0 °C

7.76E-7 Ω·m

Show Material materials with Electrical resistivity of 7.76E-7 Ω·m

200.0 °C

8.49E-7 Ω·m

Show Material materials with Electrical resistivity of 8.49E-7 Ω·m

300.0 °C

9.14E-7 Ω·m

Show Material materials with Electrical resistivity of 9.14E-7 Ω·m

400.0 °C

9.71E-7 Ω·m

Show Material materials with Electrical resistivity of 9.71E-7 Ω·m

500.0 °C

1.02E-6 Ω·m

Show Material materials with Electrical resistivity of 1.02E-6 Ω·m

600.0 °C

1.07E-6 Ω·m

Show Material materials with Electrical resistivity of 1.07E-6 Ω·m

700.0 °C

1.1E-6 Ω·m

Show Material materials with Electrical resistivity of 1.1E-6 Ω·m

800.0 °C

1.14E-6 Ω·m

Show Material materials with Electrical resistivity of 1.14E-6 Ω·m

900.0 °C

1.17E-6 Ω·m

Show Material materials with Electrical resistivity of 1.17E-6 Ω·m

1000.0 °C

1.19E-6 Ω·m

Show Material materials with Electrical resistivity of 1.19E-6 Ω·m

Unlock all property charts

Chemical properties

PropertyValue

Carbon

0.08 %

Show Material materials with Carbon of 0.08 %

Chromium

17 - 19 %

Show Material materials with Chromium of 17 - 19 %

Manganese

2 %

Show Material materials with Manganese of 2 %

Nickel

9 - 12 %

Show Material materials with Nickel of 9 - 12 %

Niobium

1 %

Show Material materials with Niobium of 1 %

Phosphorus

0.05 %

Show Material materials with Phosphorus of 0.05 %

Silicon

1 %

Show Material materials with Silicon of 1 %

Sulfur

0.015 %

Show Material materials with Sulfur of 0.015 %