EN 10217-7 Grade X1CrNiMoCuN20-18-7 solution annealed (+AT)

Want to keep this datasheet? Save it now in your required format

Description

The austenitic steel X1CrNiMoCuN20-18-7 is available in the solution annealed condition. Welded circular tubes of this steel are used for compression load and for corrosive load at room temperature, low temperatures and elevated temperatures. The material is resistant to intercrystalline corrosion (up to 400 °C) also in the welded condition.

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

8 g/cm³

Show Material materials with Density of 8 g/cm³

Mechanical

PropertyTemperatureValueComment

Elastic modulus

20.0 °C

195 GPa

Show Material materials with Elastic modulus of 195 GPa

100.0 °C

190 GPa

Show Material materials with Elastic modulus of 190 GPa

200.0 °C

182 GPa

Show Material materials with Elastic modulus of 182 GPa

300.0 °C

174 GPa

Show Material materials with Elastic modulus of 174 GPa

400.0 °C

166 GPa

Show Material materials with Elastic modulus of 166 GPa

500.0 °C

158 GPa

Show Material materials with Elastic modulus of 158 GPa

Elongation

20.0 °C

35 %

Show Material materials with Elongation of 35 %

Elongation, transverse

20.0 °C

30 %

Show Material materials with Elongation, transverse of 30 %

Poisson's ratio

23.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

Typical for Austenitic Stainless Steel

Shear modulus

23.0 °C

77 GPa

Show Material materials with Shear modulus of 77 GPa

Typical for Austenitic Stainless Steel

Tensile strength

20.0 °C

650 - 850 MPa

Show Material materials with Tensile strength of 650 - 850 MPa

Tensile strength, transverse

20.0 °C

650 - 850 MPa

Show Material materials with Tensile strength, transverse of 650 - 850 MPa

Yield strength Rp0.2

20.0 °C

300 MPa

Show Material materials with Yield strength Rp0.2 of 300 MPa

50.0 °C

267 MPa

Show Material materials with Yield strength Rp0.2 of 267 MPa

100.0 °C

230 MPa

Show Material materials with Yield strength Rp0.2 of 230 MPa

150.0 °C

205 MPa

Show Material materials with Yield strength Rp0.2 of 205 MPa

200.0 °C

190 MPa

Show Material materials with Yield strength Rp0.2 of 190 MPa

250.0 °C

180 MPa

Show Material materials with Yield strength Rp0.2 of 180 MPa

300.0 °C

170 MPa

Show Material materials with Yield strength Rp0.2 of 170 MPa

350.0 °C

165 MPa

Show Material materials with Yield strength Rp0.2 of 165 MPa

400.0 °C

160 MPa

Show Material materials with Yield strength Rp0.2 of 160 MPa

450.0 °C

153 MPa

Show Material materials with Yield strength Rp0.2 of 153 MPa

500.0 °C

148 MPa

Show Material materials with Yield strength Rp0.2 of 148 MPa

Unlock all property charts

Yield strength Rp0.2, transverse

20.0 °C

300 MPa

Show Material materials with Yield strength Rp0.2, transverse of 300 MPa

Yield strength Rp1.0

20.0 °C

340 MPa

Show Material materials with Yield strength Rp1.0 of 340 MPa

50.0 °C

306 MPa

Show Material materials with Yield strength Rp1.0 of 306 MPa

100.0 °C

270 MPa

Show Material materials with Yield strength Rp1.0 of 270 MPa

150.0 °C

245 MPa

Show Material materials with Yield strength Rp1.0 of 245 MPa

200.0 °C

225 MPa

Show Material materials with Yield strength Rp1.0 of 225 MPa

250.0 °C

212 MPa

Show Material materials with Yield strength Rp1.0 of 212 MPa

300.0 °C

200 MPa

Show Material materials with Yield strength Rp1.0 of 200 MPa

350.0 °C

195 MPa

Show Material materials with Yield strength Rp1.0 of 195 MPa

400.0 °C

190 MPa

Show Material materials with Yield strength Rp1.0 of 190 MPa

450.0 °C

184 MPa

Show Material materials with Yield strength Rp1.0 of 184 MPa

500.0 °C

180 MPa

Show Material materials with Yield strength Rp1.0 of 180 MPa

Unlock all property charts

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

100.0 °C

1.65E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.65E-5 1/K

200.0 °C

1.7E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.7E-5 1/K

300.0 °C

1.75E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.75E-5 1/K

400.0 °C

1.8E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.8E-5 1/K

500.0 °C

1.8E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.8E-5 1/K

Unlock all property charts

Melting point

1230 - 1480 °C

Show Material materials with Melting point of 1230 - 1480 °C

Typical for Austenitic Stainless Steel

Specific heat capacity

20.0 °C

500 J/(kg·K)

Show Material materials with Specific heat capacity of 500 J/(kg·K)

Thermal conductivity

20.0 °C

14 W/(m·K)

Show Material materials with Thermal conductivity of 14 W/(m·K)

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

8.5E-7 Ω·m

Show Material materials with Electrical resistivity of 8.5E-7 Ω·m

Chemical properties

PropertyValue

Carbon

0.02 %

Show Material materials with Carbon of 0.02 %

Chromium

19.5 - 20.5 %

Show Material materials with Chromium of 19.5 - 20.5 %

Copper

0.5 - 1 %

Show Material materials with Copper of 0.5 - 1 %

Manganese

1 %

Show Material materials with Manganese of 1 %

Molybdenum

6 - 7 %

Show Material materials with Molybdenum of 6 - 7 %

Nickel

17.5 - 18.5 %

Show Material materials with Nickel of 17.5 - 18.5 %

Nitrogen

0.18 - 0.25 %

Show Material materials with Nitrogen of 0.18 - 0.25 %

Phosphorus

0.03 %

Show Material materials with Phosphorus of 0.03 %

Silicon

0.7 %

Show Material materials with Silicon of 0.7 %

Sulfur

0.01 %

Show Material materials with Sulfur of 0.01 %