The heat treatable high temperature material X20CrMoV11-1, material number 1.4922 shows good high-temperature strength up to approx. 580 °C. and scaling resistance up to 700 °C. Application for components of high-temperature strength in pipeline, steam boiler and turbine construction at the upper temperature and pressure range as well as for parts in chemical industry and reactor engineering.

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

7.7 - 7.76 g/cm³

Show Material materials with Density of 7.7 - 7.76 g/cm³

50.0 °C

7.75 g/cm³

Show Material materials with Density of 7.75 g/cm³

100.0 °C

7.74 g/cm³

Show Material materials with Density of 7.74 g/cm³

150.0 °C

7.73 g/cm³

Show Material materials with Density of 7.73 g/cm³

200.0 °C

7.71 g/cm³

Show Material materials with Density of 7.71 g/cm³

250.0 °C

7.7 g/cm³

Show Material materials with Density of 7.7 g/cm³

300.0 °C

7.68 g/cm³

Show Material materials with Density of 7.68 g/cm³

350.0 °C

7.67 g/cm³

Show Material materials with Density of 7.67 g/cm³

400.0 °C

7.65 g/cm³

Show Material materials with Density of 7.65 g/cm³

450.0 °C

7.64 g/cm³

Show Material materials with Density of 7.64 g/cm³

500.0 °C

7.62 g/cm³

Show Material materials with Density of 7.62 g/cm³

550.0 °C

7.61 g/cm³

Show Material materials with Density of 7.61 g/cm³

600.0 °C

7.59 g/cm³

Show Material materials with Density of 7.59 g/cm³

Mechanical

PropertyTemperatureValue

Elastic modulus

20.0 °C

216 - 218 GPa

Show Material materials with Elastic modulus of 216 - 218 GPa

50.0 °C

216.02 GPa

Show Material materials with Elastic modulus of 216.02 GPa

100.0 °C

209 - 213 GPa

Show Material materials with Elastic modulus of 209 - 213 GPa

150.0 °C

209.64 GPa

Show Material materials with Elastic modulus of 209.64 GPa

200.0 °C

200 - 206.21 GPa

Show Material materials with Elastic modulus of 200 - 206.21 GPa

250.0 °C

202.38 GPa

Show Material materials with Elastic modulus of 202.38 GPa

300.0 °C

190 - 198.26 GPa

Show Material materials with Elastic modulus of 190 - 198.26 GPa

350.0 °C

193.94 GPa

Show Material materials with Elastic modulus of 193.94 GPa

400.0 °C

179 - 190 GPa

Show Material materials with Elastic modulus of 179 - 190 GPa

450.0 °C

184.33 GPa

Show Material materials with Elastic modulus of 184.33 GPa

500.0 °C

167 - 180 GPa

Show Material materials with Elastic modulus of 167 - 180 GPa

550.0 °C

172.85 GPa

Show Material materials with Elastic modulus of 172.85 GPa

600.0 °C

127 - 167 GPa

Show Material materials with Elastic modulus of 127 - 167 GPa

Unlock all property charts

Elongation

20.0 °C

14 - 16 %

Show Material materials with Elongation of 14 - 16 %

Poisson's ratio

20.0 °C

0.28 [-]

Show Material materials with Poisson's ratio of 0.28 [-]

50.0 °C

0.28 [-]

Show Material materials with Poisson's ratio of 0.28 [-]

100.0 °C

0.28 [-]

Show Material materials with Poisson's ratio of 0.28 [-]

150.0 °C

0.28 [-]

Show Material materials with Poisson's ratio of 0.28 [-]

200.0 °C

0.29 [-]

Show Material materials with Poisson's ratio of 0.29 [-]

250.0 °C

0.29 [-]

Show Material materials with Poisson's ratio of 0.29 [-]

300.0 °C

0.29 [-]

Show Material materials with Poisson's ratio of 0.29 [-]

350.0 °C

0.29 [-]

Show Material materials with Poisson's ratio of 0.29 [-]

400.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

450.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

500.0 °C

0.31 [-]

Show Material materials with Poisson's ratio of 0.31 [-]

550.0 °C

0.31 [-]

Show Material materials with Poisson's ratio of 0.31 [-]

600.0 °C

0.31 [-]

Show Material materials with Poisson's ratio of 0.31 [-]

Unlock all property charts

Shear modulus

20.0 °C

84.95 GPa

Show Material materials with Shear modulus of 84.95 GPa

50.0 °C

84.27 GPa

Show Material materials with Shear modulus of 84.27 GPa

100.0 °C

82.99 GPa

Show Material materials with Shear modulus of 82.99 GPa

150.0 °C

81.62 GPa

Show Material materials with Shear modulus of 81.62 GPa

200.0 °C

80.05 GPa

Show Material materials with Shear modulus of 80.05 GPa

250.0 °C

78.48 GPa

Show Material materials with Shear modulus of 78.48 GPa

300.0 °C

76.71 GPa

Show Material materials with Shear modulus of 76.71 GPa

350.0 °C

74.95 GPa

Show Material materials with Shear modulus of 74.95 GPa

400.0 °C

73.08 GPa

Show Material materials with Shear modulus of 73.08 GPa

450.0 °C

70.93 GPa

Show Material materials with Shear modulus of 70.93 GPa

500.0 °C

68.57 GPa

Show Material materials with Shear modulus of 68.57 GPa

550.0 °C

66.02 GPa

Show Material materials with Shear modulus of 66.02 GPa

600.0 °C

63.27 GPa

Show Material materials with Shear modulus of 63.27 GPa

Unlock all property charts

Tensile strength

20.0 °C

700 - 850 MPa

Show Material materials with Tensile strength of 700 - 850 MPa

Yield strength

20.0 °C

500 MPa

Show Material materials with Yield strength of 500 MPa

Yield strength Rp0.2

20.0 °C

485 MPa

Show Material materials with Yield strength Rp0.2 of 485 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

20.0 °C

1.02E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.02E-5 1/K

100.0 °C

1.05E-5 - 1.08E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.05E-5 - 1.08E-5 1/K

200.0 °C

1.09E-5 - 1.12E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.09E-5 - 1.12E-5 1/K

300.0 °C

1.13E-5 - 1.16E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.13E-5 - 1.16E-5 1/K

400.0 °C

1.16E-5 - 1.19E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.16E-5 - 1.19E-5 1/K

500.0 °C

1.2E-5 - 1.21E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.2E-5 - 1.21E-5 1/K

600.0 °C

1.22E-5 - 1.23E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.22E-5 - 1.23E-5 1/K

Unlock all property charts

Max service temperature, long

550 - 600 °C

Show Material materials with Max service temperature, long of 550 - 600 °C

Melting point

1370 - 1530 °C

Show Material materials with Melting point of 1370 - 1530 °C

Typical for Martensitic Stainless Steel

Specific heat capacity

20.0 °C

439 - 460 J/(kg·K)

Show Material materials with Specific heat capacity of 439 - 460 J/(kg·K)

100.0 °C

474 - 490 J/(kg·K)

Show Material materials with Specific heat capacity of 474 - 490 J/(kg·K)

200.0 °C

498 - 540 J/(kg·K)

Show Material materials with Specific heat capacity of 498 - 540 J/(kg·K)

300.0 °C

517 - 580 J/(kg·K)

Show Material materials with Specific heat capacity of 517 - 580 J/(kg·K)

400.0 °C

538 - 630 J/(kg·K)

Show Material materials with Specific heat capacity of 538 - 630 J/(kg·K)

500.0 °C

564 - 710 J/(kg·K)

Show Material materials with Specific heat capacity of 564 - 710 J/(kg·K)

600.0 °C

598 - 830 J/(kg·K)

Show Material materials with Specific heat capacity of 598 - 830 J/(kg·K)

Unlock all property charts

Thermal conductivity

20.0 °C

24 W/(m·K)

Show Material materials with Thermal conductivity of 24 W/(m·K)

100.0 °C

24 - 24.4 W/(m·K)

Show Material materials with Thermal conductivity of 24 - 24.4 W/(m·K)

200.0 °C

24.8 - 25 W/(m·K)

Show Material materials with Thermal conductivity of 24.8 - 25 W/(m·K)

300.0 °C

25 - 25.1 W/(m·K)

Show Material materials with Thermal conductivity of 25 - 25.1 W/(m·K)

400.0 °C

25.6 - 26 W/(m·K)

Show Material materials with Thermal conductivity of 25.6 - 26 W/(m·K)

500.0 °C

26 - 26.1 W/(m·K)

Show Material materials with Thermal conductivity of 26 - 26.1 W/(m·K)

600.0 °C

26 - 26.4 W/(m·K)

Show Material materials with Thermal conductivity of 26 - 26.4 W/(m·K)

650.0 °C

30 W/(m·K)

Show Material materials with Thermal conductivity of 30 W/(m·K)

Unlock all property charts

Thermal diffusivity

20.0 °C

7.1 mm²/s

Show Material materials with Thermal diffusivity of 7.1 mm²/s

100.0 °C

6.3 mm²/s

Show Material materials with Thermal diffusivity of 6.3 mm²/s

200.0 °C

6 mm²/s

Show Material materials with Thermal diffusivity of 6 mm²/s

300.0 °C

5.7 mm²/s

Show Material materials with Thermal diffusivity of 5.7 mm²/s

400.0 °C

5.4 mm²/s

Show Material materials with Thermal diffusivity of 5.4 mm²/s

500.0 °C

4.9 mm²/s

Show Material materials with Thermal diffusivity of 4.9 mm²/s

600.0 °C

4.1 mm²/s

Show Material materials with Thermal diffusivity of 4.1 mm²/s

Unlock all property charts

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

6E-7 - 6.03E-7 Ω·m

Show Material materials with Electrical resistivity of 6E-7 - 6.03E-7 Ω·m

50.0 °C

6.26E-7 Ω·m

Show Material materials with Electrical resistivity of 6.26E-7 Ω·m

100.0 °C

6.68E-7 - 6.7E-7 Ω·m

Show Material materials with Electrical resistivity of 6.68E-7 - 6.7E-7 Ω·m

150.0 °C

7.06E-7 Ω·m

Show Material materials with Electrical resistivity of 7.06E-7 Ω·m

200.0 °C

7.4E-7 - 7.43E-7 Ω·m

Show Material materials with Electrical resistivity of 7.4E-7 - 7.43E-7 Ω·m

250.0 °C

7.83E-7 Ω·m

Show Material materials with Electrical resistivity of 7.83E-7 Ω·m

300.0 °C

8.17E-7 - 8.2E-7 Ω·m

Show Material materials with Electrical resistivity of 8.17E-7 - 8.2E-7 Ω·m

350.0 °C

8.54E-7 Ω·m

Show Material materials with Electrical resistivity of 8.54E-7 Ω·m

400.0 °C

8.9E-7 Ω·m

Show Material materials with Electrical resistivity of 8.9E-7 Ω·m

450.0 °C

9.25E-7 Ω·m

Show Material materials with Electrical resistivity of 9.25E-7 Ω·m

500.0 °C

9.6E-7 - 9.62E-7 Ω·m

Show Material materials with Electrical resistivity of 9.6E-7 - 9.62E-7 Ω·m

550.0 °C

9.99E-7 Ω·m

Show Material materials with Electrical resistivity of 9.99E-7 Ω·m

600.0 °C

1.03E-6 - 1.04E-6 Ω·m

Show Material materials with Electrical resistivity of 1.03E-6 - 1.04E-6 Ω·m

Unlock all property charts

Chemical properties

PropertyValue

Carbon

0.17 - 0.23 %

Show Material materials with Carbon of 0.17 - 0.23 %

Chromium

10 - 12.5 %

Show Material materials with Chromium of 10 - 12.5 %

Manganese

0.3 - 1 %

Show Material materials with Manganese of 0.3 - 1 %

Molybdenum

0.8 - 1.2 %

Show Material materials with Molybdenum of 0.8 - 1.2 %

Nickel

0.3 - 0.8 %

Show Material materials with Nickel of 0.3 - 0.8 %

Phosphorus

0.02 - 0.03 %

Show Material materials with Phosphorus of 0.02 - 0.03 %

Silicon

0.4 %

Show Material materials with Silicon of 0.4 %

Sulfur

0.005 - 0.015 %

Show Material materials with Sulfur of 0.005 - 0.015 %

Vanadium

0.2 - 0.35 %

Show Material materials with Vanadium of 0.2 - 0.35 %