EN 10272 Grade X2CrNiMoN17-11-2 solution annealed (+AT)

Want to keep this datasheet? Save it now in your required format

Description

The austenitic steel grade X2CrNiMoN17-11-2 acc. to DIN EN 10272 : 2001-01is used for hot and cold formed rods for pressure vessels. The material shows higher strength and structure stability by N-addition. It has high resistance to oxidizing media. its interaction parameter (Pitting index) is increased by N. The steel is suitabable for mirror finishing and resistant to selective attacks particularly and in welded condition good corrosion resistant. The material shows resistance to intercrystalline corrosion also in sensitized condition.

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

7.96 - 8 g/cm³

Show Material materials with Density of 7.96 - 8 g/cm³

Mechanical

PropertyTemperatureValueComment

Elastic modulus

-100.0 °C

206 GPa

Show Material materials with Elastic modulus of 206 GPa

20.0 °C

196 - 200 GPa

Show Material materials with Elastic modulus of 196 - 200 GPa

100.0 °C

190 - 194 GPa

Show Material materials with Elastic modulus of 190 - 194 GPa

200.0 °C

182 - 186 GPa

Show Material materials with Elastic modulus of 182 - 186 GPa

300.0 °C

174 - 179 GPa

Show Material materials with Elastic modulus of 174 - 179 GPa

400.0 °C

166 - 172 GPa

Show Material materials with Elastic modulus of 166 - 172 GPa

500.0 °C

158 - 165 GPa

Show Material materials with Elastic modulus of 158 - 165 GPa

600.0 °C

150 GPa

Show Material materials with Elastic modulus of 150 GPa

700.0 °C

142 GPa

Show Material materials with Elastic modulus of 142 GPa

800.0 °C

134 GPa

Show Material materials with Elastic modulus of 134 GPa

900.0 °C

127 GPa

Show Material materials with Elastic modulus of 127 GPa

1000.0 °C

120 GPa

Show Material materials with Elastic modulus of 120 GPa

Elongation

20.0 °C

40 %

Show Material materials with Elongation of 40 %

Elongation, transverse

20.0 °C

30 %

Show Material materials with Elongation, transverse of 30 %

Hardness, Brinell

20.0 °C

250 [-]

Show Material materials with Hardness, Brinell of 250 [-]

Hardness, Brinell, trans

20.0 °C

250 [-]

Show Material materials with Hardness, Brinell, trans of 250 [-]

Poisson's ratio

23.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

Typical for Austenitic Stainless Steel

Shear modulus

23.0 °C

77 GPa

Show Material materials with Shear modulus of 77 GPa

Typical for Austenitic Stainless Steel

Tensile strength

20.0 °C

580 - 800 MPa

Show Material materials with Tensile strength of 580 - 800 MPa

100.0 °C

520 MPa

Show Material materials with Tensile strength of 520 MPa

150.0 °C

490 MPa

Show Material materials with Tensile strength of 490 MPa

200.0 °C

460 MPa

Show Material materials with Tensile strength of 460 MPa

250.0 °C

450 MPa

Show Material materials with Tensile strength of 450 MPa

300.0 °C

440 MPa

Show Material materials with Tensile strength of 440 MPa

350.0 °C

435 MPa

Show Material materials with Tensile strength of 435 MPa

Unlock all property charts

Tensile strength, transverse

20.0 °C

580 - 800 MPa

Show Material materials with Tensile strength, transverse of 580 - 800 MPa

Yield strength Rp0.2

20.0 °C

280 MPa

Show Material materials with Yield strength Rp0.2 of 280 MPa

100.0 °C

215 MPa

Show Material materials with Yield strength Rp0.2 of 215 MPa

150.0 °C

195 MPa

Show Material materials with Yield strength Rp0.2 of 195 MPa

200.0 °C

175 MPa

Show Material materials with Yield strength Rp0.2 of 175 MPa

250.0 °C

165 MPa

Show Material materials with Yield strength Rp0.2 of 165 MPa

300.0 °C

155 MPa

Show Material materials with Yield strength Rp0.2 of 155 MPa

350.0 °C

150 MPa

Show Material materials with Yield strength Rp0.2 of 150 MPa

400.0 °C

145 MPa

Show Material materials with Yield strength Rp0.2 of 145 MPa

450.0 °C

140 MPa

Show Material materials with Yield strength Rp0.2 of 140 MPa

500.0 °C

138 MPa

Show Material materials with Yield strength Rp0.2 of 138 MPa

550.0 °C

136 MPa

Show Material materials with Yield strength Rp0.2 of 136 MPa

Unlock all property charts

Yield strength Rp0.2, transverse

20.0 °C

280 MPa

Show Material materials with Yield strength Rp0.2, transverse of 280 MPa

Yield strength Rp1.0

20.0 °C

315 MPa

Show Material materials with Yield strength Rp1.0 of 315 MPa

100.0 °C

245 MPa

Show Material materials with Yield strength Rp1.0 of 245 MPa

150.0 °C

225 MPa

Show Material materials with Yield strength Rp1.0 of 225 MPa

200.0 °C

205 MPa

Show Material materials with Yield strength Rp1.0 of 205 MPa

250.0 °C

195 MPa

Show Material materials with Yield strength Rp1.0 of 195 MPa

300.0 °C

185 MPa

Show Material materials with Yield strength Rp1.0 of 185 MPa

350.0 °C

180 MPa

Show Material materials with Yield strength Rp1.0 of 180 MPa

400.0 °C

175 MPa

Show Material materials with Yield strength Rp1.0 of 175 MPa

450.0 °C

170 MPa

Show Material materials with Yield strength Rp1.0 of 170 MPa

500.0 °C

168 MPa

Show Material materials with Yield strength Rp1.0 of 168 MPa

550.0 °C

166 MPa

Show Material materials with Yield strength Rp1.0 of 166 MPa

Unlock all property charts

Yield strength Rp1.0, transverse

20.0 °C

315 MPa

Show Material materials with Yield strength Rp1.0, transverse of 315 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

-100.0 °C

1.49E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.49E-5 1/K

20.0 °C

1.61E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.61E-5 1/K

100.0 °C

1.6E-5 - 1.67E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.6E-5 - 1.67E-5 1/K

200.0 °C

1.65E-5 - 1.72E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.65E-5 - 1.72E-5 1/K

300.0 °C

1.7E-5 - 1.77E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.7E-5 - 1.77E-5 1/K

400.0 °C

1.75E-5 - 1.81E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.75E-5 - 1.81E-5 1/K

500.0 °C

1.8E-5 - 1.84E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.8E-5 - 1.84E-5 1/K

600.0 °C

1.88E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.88E-5 1/K

700.0 °C

1.91E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.91E-5 1/K

800.0 °C

1.94E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.94E-5 1/K

900.0 °C

1.97E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.97E-5 1/K

1000.0 °C

2E-5 1/K

Show Material materials with Coefficient of thermal expansion of 2E-5 1/K

Unlock all property charts

Melting point

1230 - 1480 °C

Show Material materials with Melting point of 1230 - 1480 °C

Typical for Austenitic Stainless Steel

Specific heat capacity

-100.0 °C

440 J/(kg·K)

Show Material materials with Specific heat capacity of 440 J/(kg·K)

20.0 °C

472 - 500 J/(kg·K)

Show Material materials with Specific heat capacity of 472 - 500 J/(kg·K)

100.0 °C

487 J/(kg·K)

Show Material materials with Specific heat capacity of 487 J/(kg·K)

200.0 °C

503 J/(kg·K)

Show Material materials with Specific heat capacity of 503 J/(kg·K)

300.0 °C

512 J/(kg·K)

Show Material materials with Specific heat capacity of 512 J/(kg·K)

400.0 °C

520 J/(kg·K)

Show Material materials with Specific heat capacity of 520 J/(kg·K)

500.0 °C

530 J/(kg·K)

Show Material materials with Specific heat capacity of 530 J/(kg·K)

600.0 °C

541 J/(kg·K)

Show Material materials with Specific heat capacity of 541 J/(kg·K)

700.0 °C

551 J/(kg·K)

Show Material materials with Specific heat capacity of 551 J/(kg·K)

800.0 °C

559 J/(kg·K)

Show Material materials with Specific heat capacity of 559 J/(kg·K)

900.0 °C

565 J/(kg·K)

Show Material materials with Specific heat capacity of 565 J/(kg·K)

1000.0 °C

571 J/(kg·K)

Show Material materials with Specific heat capacity of 571 J/(kg·K)

Unlock all property charts

Thermal conductivity

20.0 °C

13.3 - 15 W/(m·K)

Show Material materials with Thermal conductivity of 13.3 - 15 W/(m·K)

100.0 °C

14.9 W/(m·K)

Show Material materials with Thermal conductivity of 14.9 W/(m·K)

200.0 °C

16.5 W/(m·K)

Show Material materials with Thermal conductivity of 16.5 W/(m·K)

300.0 °C

18.1 W/(m·K)

Show Material materials with Thermal conductivity of 18.1 W/(m·K)

400.0 °C

19.5 W/(m·K)

Show Material materials with Thermal conductivity of 19.5 W/(m·K)

500.0 °C

21 W/(m·K)

Show Material materials with Thermal conductivity of 21 W/(m·K)

600.0 °C

22.4 W/(m·K)

Show Material materials with Thermal conductivity of 22.4 W/(m·K)

700.0 °C

23.8 W/(m·K)

Show Material materials with Thermal conductivity of 23.8 W/(m·K)

800.0 °C

25.2 W/(m·K)

Show Material materials with Thermal conductivity of 25.2 W/(m·K)

Unlock all property charts

Thermal diffusivity

20.0 °C

3.5 mm²/s

Show Material materials with Thermal diffusivity of 3.5 mm²/s

100.0 °C

3.8 mm²/s

Show Material materials with Thermal diffusivity of 3.8 mm²/s

200.0 °C

4 mm²/s

Show Material materials with Thermal diffusivity of 4 mm²/s

300.0 °C

4.3 mm²/s

Show Material materials with Thermal diffusivity of 4.3 mm²/s

400.0 °C

4.5 mm²/s

Show Material materials with Thermal diffusivity of 4.5 mm²/s

500.0 °C

4.7 mm²/s

Show Material materials with Thermal diffusivity of 4.7 mm²/s

600.0 °C

4.8 mm²/s

Show Material materials with Thermal diffusivity of 4.8 mm²/s

700.0 °C

5.1 mm²/s

Show Material materials with Thermal diffusivity of 5.1 mm²/s

800.0 °C

5.4 mm²/s

Show Material materials with Thermal diffusivity of 5.4 mm²/s

Unlock all property charts

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

7.5E-7 - 7.91E-7 Ω·m

Show Material materials with Electrical resistivity of 7.5E-7 - 7.91E-7 Ω·m

100.0 °C

8.45E-7 Ω·m

Show Material materials with Electrical resistivity of 8.45E-7 Ω·m

200.0 °C

9.19E-7 Ω·m

Show Material materials with Electrical resistivity of 9.19E-7 Ω·m

300.0 °C

9.77E-7 Ω·m

Show Material materials with Electrical resistivity of 9.77E-7 Ω·m

400.0 °C

1.03E-6 Ω·m

Show Material materials with Electrical resistivity of 1.03E-6 Ω·m

500.0 °C

1.08E-6 Ω·m

Show Material materials with Electrical resistivity of 1.08E-6 Ω·m

600.0 °C

1.12E-6 Ω·m

Show Material materials with Electrical resistivity of 1.12E-6 Ω·m

700.0 °C

1.15E-6 Ω·m

Show Material materials with Electrical resistivity of 1.15E-6 Ω·m

800.0 °C

1.18E-6 Ω·m

Show Material materials with Electrical resistivity of 1.18E-6 Ω·m

Unlock all property charts

Chemical properties

PropertyValue

Carbon

0.03 %

Show Material materials with Carbon of 0.03 %

Chromium

16.5 - 18.5 %

Show Material materials with Chromium of 16.5 - 18.5 %

Manganese

2 %

Show Material materials with Manganese of 2 %

Molybdenum

2 - 2.5 %

Show Material materials with Molybdenum of 2 - 2.5 %

Nickel

10 - 12.5 %

Show Material materials with Nickel of 10 - 12.5 %

Nitrogen

0.12 - 0.22 %

Show Material materials with Nitrogen of 0.12 - 0.22 %

Phosphorus

0.05 %

Show Material materials with Phosphorus of 0.05 %

Silicon

1 %

Show Material materials with Silicon of 1 %

Sulfur

0.015 - 0.03 %

Show Material materials with Sulfur of 0.015 - 0.03 %