General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Density | 20 °C | 7.84 g/cm³ Show Material materials with Density of 7.84 g/cm³ | quenched and tempered (+QT) | EN 10025-6, EN 10137-2 | Flat |
Mechanical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elastic modulus | 20 °C | 210 GPa Show Material materials with Elastic modulus of 210 GPa | quenched and tempered (+QT) | EN 10025-6, EN 10137-2 | Flat | |
Elongation | 13.0 % Show Material materials with Elongation of 13.0 % | Predicted Value, A200 | ||||
13.4 % Show Material materials with Elongation of 13.4 % | Predicted Value, A80 | |||||
18.4 % Show Material materials with Elongation of 18.4 % | Predicted Value, A80 Transverse | |||||
18.8 % Show Material materials with Elongation of 18.8 % | Predicted Value, A5 | |||||
19.9 % Show Material materials with Elongation of 19.9 % | Predicted Value, A50 | |||||
20 °C | 16 % Show Material materials with Elongation of 16 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, VdTÜV WB 257 | Sheet, Flat | ||
20 °C | 18 % Show Material materials with Elongation of 18 % | quenched and tempered (+QT) | EN 10137-2 | Sheet, Flat | Transverse | |
Poisson's ratio | 0.3 [-] Show Material materials with Poisson's ratio of 0.3 [-] | Typical for Steel | ||||
Reduction of area | 40.1 % Show Material materials with Reduction of area of 40.1 % | Predicted Value | ||||
44.7 % Show Material materials with Reduction of area of 44.7 % | Predicted Value, Transverse | |||||
Shear modulus | 20 °C | 80 GPa Show Material materials with Shear modulus of 80 GPa | quenched and tempered (+QT) | EN 10025-6, EN 10137-2 | Flat | |
Shear strength | 589.7 MPa Show Material materials with Shear strength of 589.7 MPa | Predicted Value | ||||
Tensile strength | 20 °C | 590 - 820 MPa Show Material materials with Tensile strength of 590 - 820 MPa | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, VdTÜV WB 257 | Sheet, Flat | |
20 °C | 590 - 770 MPa Show Material materials with Tensile strength of 590 - 770 MPa | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, VdTÜV WB 257 | Sheet, Flat | ||
20 °C | 640 - 820 MPa Show Material materials with Tensile strength of 640 - 820 MPa | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, VdTÜV WB 257 | Sheet, Flat | ||
20 °C | 640 - 770 MPa Show Material materials with Tensile strength of 640 - 770 MPa | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, VdTÜV WB 257 | Sheet, Flat | ||
20 °C | 640 - 820 MPa Show Material materials with Tensile strength of 640 - 820 MPa | quenched and tempered (+QT) | EN 10137-2 | Sheet, Flat | Transverse | |
Yield strength | 302.8 MPa Show Material materials with Yield strength of 302.8 MPa | Predicted Value, RP1 | ||||
329.7 MPa Show Material materials with Yield strength of 329.7 MPa | Predicted Value, RP1 Transverse | |||||
493 MPa Show Material materials with Yield strength of 493 MPa | Predicted Value, RP02 Transverse | |||||
541.7 MPa Show Material materials with Yield strength of 541.7 MPa | Predicted Value, RP05 | |||||
623.6 MPa Show Material materials with Yield strength of 623.6 MPa | Predicted Value, RP002 | |||||
20 °C | 490 MPa Show Material materials with Yield strength of 490 MPa | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, VdTÜV WB 257 | Sheet, Flat | ||
20 °C | 530 MPa Show Material materials with Yield strength of 530 MPa | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, VdTÜV WB 257 | Sheet, Flat | ||
20 °C | 550 MPa Show Material materials with Yield strength of 550 MPa | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, VdTÜV WB 257 | Sheet, Flat | ||
20 °C | 550 MPa Show Material materials with Yield strength of 550 MPa | quenched and tempered (+QT) | EN 10137-2 | Sheet, Flat | Transverse | |
100 °C | 530 MPa Show Material materials with Yield strength of 530 MPa | quenched and tempered (+QT) | EN 10137-2 | Sheet, Flat | RP02 | |
150 °C | 510 MPa Show Material materials with Yield strength of 510 MPa | quenched and tempered (+QT) | EN 10137-2 | Sheet, Flat | RP02 | |
200 °C | 475 MPa Show Material materials with Yield strength of 475 MPa | quenched and tempered (+QT) | EN 10137-2 | Sheet, Flat | RP02 | |
250 °C | 455 MPa Show Material materials with Yield strength of 455 MPa | quenched and tempered (+QT) | EN 10137-2 | Sheet, Flat | RP02 | |
300 °C | 440 MPa Show Material materials with Yield strength of 440 MPa | quenched and tempered (+QT) | EN 10137-2 | Sheet, Flat | RP02 | |
350 °C | 425 MPa Show Material materials with Yield strength of 425 MPa | quenched and tempered (+QT) | EN 10137-2 | Sheet, Flat | RP02 | |
400 °C | 410 MPa Show Material materials with Yield strength of 410 MPa | quenched and tempered (+QT) | EN 10137-2 | Sheet, Flat | RP02 |
Thermal
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Coefficient of thermal expansion | 100 °C | 1.2e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.2e-05 1/K | quenched and tempered (+QT) | EN 10025-6, EN 10137-2 | Flat |
Specific heat capacity | 20 °C | 430 J/(kg·K) Show Material materials with Specific heat capacity of 430 J/(kg·K) | quenched and tempered (+QT) | EN 10025-6, EN 10137-2 | Flat |
Thermal conductivity | 20 °C | 39 W/(m·K) Show Material materials with Thermal conductivity of 39 W/(m·K) | quenched and tempered (+QT) | EN 10025-6, EN 10137-2 | Flat |
Electrical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Electrical conductivity | 5 S/m Show Material materials with Electrical conductivity of 5 S/m | Predicted Value | ||||
Electrical resistivity | 20 °C | 2.7e-07 Ω·m Show Material materials with Electrical resistivity of 2.7e-07 Ω·m | quenched and tempered (+QT) | EN 10025-6, EN 10137-2 | Flat |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | 0.015 % Show Material materials with Aluminium of 0.015 % | quenched and tempered (+QT) | EN 10137-2 | Sheet, Flat |
Boron | 0.005 % Show Material materials with Boron of 0.005 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, VdTÜV WB 257 | Sheet, Flat |
Carbon | 0.2 % Show Material materials with Carbon of 0.2 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, VdTÜV WB 257 | Sheet, Flat |
Chromium | 1.5 % Show Material materials with Chromium of 1.5 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, VdTÜV WB 257 | Sheet, Flat |
Copper | 0.5 % Show Material materials with Copper of 0.5 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, VdTÜV WB 257 | Sheet, Flat |
Manganese | 1.6 % Show Material materials with Manganese of 1.6 % | quenched and tempered (+QT) | EN 10137-2 | Sheet, Flat |
1.7 % Show Material materials with Manganese of 1.7 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, VdTÜV WB 257 | Sheet, Flat | |
Molybdenum | 0.6 % Show Material materials with Molybdenum of 0.6 % | quenched and tempered (+QT) | EN 10137-2 | Sheet, Flat |
0.7 % Show Material materials with Molybdenum of 0.7 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, VdTÜV WB 257 | Sheet, Flat | |
Nickel | 2 % Show Material materials with Nickel of 2 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, VdTÜV WB 257 | Sheet, Flat |
Niobium | 0.06 % Show Material materials with Niobium of 0.06 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, VdTÜV WB 257 | Sheet, Flat |
Nitrogen | 0.015 % Show Material materials with Nitrogen of 0.015 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, VdTÜV WB 257 | Sheet, Flat |
Phosphorus | 0.02 % Show Material materials with Phosphorus of 0.02 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, VdTÜV WB 257 | Sheet, Flat |
Silicon | 0.8 % Show Material materials with Silicon of 0.8 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, VdTÜV WB 257 | Sheet, Flat |
Sulfur | 0.01 % Show Material materials with Sulfur of 0.01 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, VdTÜV WB 257 | Sheet, Flat |
Titanium | 0.05 % Show Material materials with Titanium of 0.05 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, VdTÜV WB 257 | Sheet, Flat |
Vanadium | 0.12 % Show Material materials with Vanadium of 0.12 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, VdTÜV WB 257 | Sheet, Flat |
Zirconium | 0.12 % Show Material materials with Zirconium of 0.12 % | quenched and tempered (+QT) | EN 10137-2 | Sheet, Flat |
0.15 % Show Material materials with Zirconium of 0.15 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, VdTÜV WB 257 | Sheet, Flat |
Technological properties
Property | ||
---|---|---|
Supplier Disclaimer | The given information is a rough description and some properties can depend on various factors such as product thickness. Please contact the supplier or refer to the related norm or standard for further information. |
Do you have a technical question or need more information about this material?
Post it as a comment below and receive answers from engineers and other community members.