EN 10025-6 Grade S690QL1 quenched and tempered (+QT)

View all suppliers (6)

Want to keep this datasheet? Save it now in your required format

Description

S690QL1 is a tempered and weldable fine grained steel. yield point: >690 N/mm² application: welded steel constructions of various types, e.g. bridges and load-carrying constructions as well as transport vehicles, lifting and earthmoving machines. application limits: at -60°C is warranted a notch impact energy of 30 J (longitudinal test specimen) cold formability: for nominal size < 16 mm bending radius in transversal direction 3xs in longitudinal direction 4xs (s= nominal thickness) hot forming property: allowed only for stress relieve annealing temperature (max. 580°C) suitability for welding: Steel is weldable according to the common welding methods (EURONORM-INFORMATION Nr. 2 has to be considered)

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

"Typical" values were obtained via a literature search. "Predicted" values were imputed via artificial intelligence technology. While we have placed significant efforts in ensuring data accuracy, "typical" and "predicted" data should be considered indicative and verified by appropriate material testing. Please do contact us if additional information on the the predicted data method is required.
All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

20 °C

7.84 g/cm³

Show Material materials with Density of 7.84 g/cm³

quenched and tempered (+QT)

EN 10025-6, EN 10137-2

Flat

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Elastic modulus

20 °C

210 GPa

Show Material materials with Elastic modulus of 210 GPa

quenched and tempered (+QT)

EN 10025-6, EN 10137-2

Flat

100 °C

205 GPa

Show Material materials with Elastic modulus of 205 GPa

quenched and tempered (+QT)

EN 10025-6, EN 10137-2

Flat

200 °C

198 GPa

Show Material materials with Elastic modulus of 198 GPa

quenched and tempered (+QT)

EN 10025-6, EN 10137-2

Flat

300 °C

190 GPa

Show Material materials with Elastic modulus of 190 GPa

quenched and tempered (+QT)

EN 10025-6, EN 10137-2

Flat

400 °C

182 GPa

Show Material materials with Elastic modulus of 182 GPa

quenched and tempered (+QT)

EN 10025-6, EN 10137-2

Flat

500 °C

173 GPa

Show Material materials with Elastic modulus of 173 GPa

quenched and tempered (+QT)

EN 10025-6, EN 10137-2

Flat

Elongation

12.1 %

Show Material materials with Elongation of 12.1 %

Predicted Value, A80

12.7 %

Show Material materials with Elongation of 12.7 %

Predicted Value, A200

17.9 %

Show Material materials with Elongation of 17.9 %

Predicted Value, A5

18.2 %

Show Material materials with Elongation of 18.2 %

Predicted Value, A50

18.3 %

Show Material materials with Elongation of 18.3 %

Predicted Value, A80 Transverse

20 °C

14 %

Show Material materials with Elongation of 14 %

quenched and tempered (+QT)

EN 10137-2, EN 10025-6, VdTÜV WB 257

Sheet, Flat

20 °C

16 %

Show Material materials with Elongation of 16 %

quenched and tempered (+QT)

EN 10137-2

Sheet, Flat

Transverse

Poisson's ratio

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

Typical for Steel

Reduction of area

40.2 %

Show Material materials with Reduction of area of 40.2 %

Predicted Value

44.8 %

Show Material materials with Reduction of area of 44.8 %

Predicted Value, Transverse

Shear modulus

79.6 GPa

Show Material materials with Shear modulus of 79.6 GPa

Predicted Value

Shear strength

600.6 MPa

Show Material materials with Shear strength of 600.6 MPa

Predicted Value

Tensile strength

20 °C

710 - 940 MPa

Show Material materials with Tensile strength of 710 - 940 MPa

quenched and tempered (+QT)

EN 10137-2, EN 10025-6, VdTÜV WB 257

Sheet, Flat

20 °C

710 - 930 MPa

Show Material materials with Tensile strength of 710 - 930 MPa

quenched and tempered (+QT)

EN 10137-2, EN 10025-6, VdTÜV WB 257

Sheet, Flat

20 °C

710 - 900 MPa

Show Material materials with Tensile strength of 710 - 900 MPa

quenched and tempered (+QT)

EN 10137-2, EN 10025-6, VdTÜV WB 257

Sheet, Flat

20 °C

760 - 940 MPa

Show Material materials with Tensile strength of 760 - 940 MPa

quenched and tempered (+QT)

EN 10137-2, EN 10025-6, VdTÜV WB 257

Sheet, Flat

20 °C

760 - 930 MPa

Show Material materials with Tensile strength of 760 - 930 MPa

quenched and tempered (+QT)

EN 10137-2, EN 10025-6, VdTÜV WB 257

Sheet, Flat

20 °C

760 - 900 MPa

Show Material materials with Tensile strength of 760 - 900 MPa

quenched and tempered (+QT)

EN 10137-2, EN 10025-6, VdTÜV WB 257

Sheet, Flat

20 °C

770 - 940 MPa

Show Material materials with Tensile strength of 770 - 940 MPa

quenched and tempered (+QT)

EN 10137-2, EN 10025-6, VdTÜV WB 257

Sheet, Flat

20 °C

770 - 930 MPa

Show Material materials with Tensile strength of 770 - 930 MPa

quenched and tempered (+QT)

EN 10137-2, EN 10025-6, VdTÜV WB 257

Sheet, Flat

20 °C

770 - 900 MPa

Show Material materials with Tensile strength of 770 - 900 MPa

quenched and tempered (+QT)

EN 10137-2, EN 10025-6, VdTÜV WB 257

Sheet, Flat

20 °C

770 - 940 MPa

Show Material materials with Tensile strength of 770 - 940 MPa

quenched and tempered (+QT)

EN 10137-2

Sheet, Flat

Transverse

Yield strength

308.9 MPa

Show Material materials with Yield strength of 308.9 MPa

Predicted Value, RP1

329.7 MPa

Show Material materials with Yield strength of 329.7 MPa

Predicted Value, RP1 Transverse

502.3 MPa

Show Material materials with Yield strength of 502.3 MPa

Predicted Value, RP02 Transverse

541.7 MPa

Show Material materials with Yield strength of 541.7 MPa

Predicted Value, RP05

723 MPa

Show Material materials with Yield strength of 723 MPa

Predicted Value, RP002

20 °C

630 MPa

Show Material materials with Yield strength of 630 MPa

quenched and tempered (+QT)

EN 10137-2, EN 10025-6, VdTÜV WB 257

Sheet, Flat

20 °C

650 MPa

Show Material materials with Yield strength of 650 MPa

quenched and tempered (+QT)

EN 10137-2, EN 10025-6, VdTÜV WB 257

Sheet, Flat

20 °C

690 MPa

Show Material materials with Yield strength of 690 MPa

quenched and tempered (+QT)

EN 10137-2, EN 10025-6, VdTÜV WB 257

Sheet, Flat

20 °C

690 MPa

Show Material materials with Yield strength of 690 MPa

quenched and tempered (+QT)

EN 10137-2

Sheet, Flat

Transverse

100 °C

660 MPa

Show Material materials with Yield strength of 660 MPa

quenched and tempered (+QT)

EN 10137-2

Sheet, Flat

RP02

150 °C

640 MPa

Show Material materials with Yield strength of 640 MPa

quenched and tempered (+QT)

EN 10137-2

Sheet, Flat

RP02

200 °C

605 MPa

Show Material materials with Yield strength of 605 MPa

quenched and tempered (+QT)

EN 10137-2

Sheet, Flat

RP02

250 °C

585 MPa

Show Material materials with Yield strength of 585 MPa

quenched and tempered (+QT)

EN 10137-2

Sheet, Flat

RP02

300 °C

570 MPa

Show Material materials with Yield strength of 570 MPa

quenched and tempered (+QT)

EN 10137-2

Sheet, Flat

RP02

350 °C

550 MPa

Show Material materials with Yield strength of 550 MPa

quenched and tempered (+QT)

EN 10137-2

Sheet, Flat

RP02

400 °C

530 MPa

Show Material materials with Yield strength of 530 MPa

quenched and tempered (+QT)

EN 10137-2

Sheet, Flat

RP02

Thermal

PropertyTemperatureValueConditionRelated StandardsShape

Coefficient of thermal expansion

100 °C

1.2e-05 1/K

Show Material materials with Coefficient of thermal expansion of 1.2e-05 1/K

quenched and tempered (+QT)

EN 10025-6, EN 10137-2

Flat

200 °C

1.3e-05 1/K

Show Material materials with Coefficient of thermal expansion of 1.3e-05 1/K

quenched and tempered (+QT)

EN 10025-6, EN 10137-2

Flat

300 °C

1.3e-05 1/K

Show Material materials with Coefficient of thermal expansion of 1.3e-05 1/K

quenched and tempered (+QT)

EN 10025-6, EN 10137-2

Flat

400 °C

1.4e-05 1/K

Show Material materials with Coefficient of thermal expansion of 1.4e-05 1/K

quenched and tempered (+QT)

EN 10025-6, EN 10137-2

Flat

500 °C

1.4e-05 1/K

Show Material materials with Coefficient of thermal expansion of 1.4e-05 1/K

quenched and tempered (+QT)

EN 10025-6, EN 10137-2

Flat

Specific heat capacity

20 °C

430 J/(kg·K)

Show Material materials with Specific heat capacity of 430 J/(kg·K)

quenched and tempered (+QT)

EN 10025-6, EN 10137-2

Flat

100 °C

470 J/(kg·K)

Show Material materials with Specific heat capacity of 470 J/(kg·K)

quenched and tempered (+QT)

EN 10025-6, EN 10137-2

Flat

200 °C

500 J/(kg·K)

Show Material materials with Specific heat capacity of 500 J/(kg·K)

quenched and tempered (+QT)

EN 10025-6, EN 10137-2

Flat

300 °C

520 J/(kg·K)

Show Material materials with Specific heat capacity of 520 J/(kg·K)

quenched and tempered (+QT)

EN 10025-6, EN 10137-2

Flat

400 °C

540 J/(kg·K)

Show Material materials with Specific heat capacity of 540 J/(kg·K)

quenched and tempered (+QT)

EN 10025-6, EN 10137-2

Flat

500 °C

570 J/(kg·K)

Show Material materials with Specific heat capacity of 570 J/(kg·K)

quenched and tempered (+QT)

EN 10025-6, EN 10137-2

Flat

Thermal conductivity

20 °C

38 W/(m·K)

Show Material materials with Thermal conductivity of 38 W/(m·K)

quenched and tempered (+QT)

EN 10025-6, EN 10137-2

Flat

100 °C

39 W/(m·K)

Show Material materials with Thermal conductivity of 39 W/(m·K)

quenched and tempered (+QT)

EN 10025-6, EN 10137-2

Flat

200 °C

40 W/(m·K)

Show Material materials with Thermal conductivity of 40 W/(m·K)

quenched and tempered (+QT)

EN 10025-6, EN 10137-2

Flat

300 °C

40 W/(m·K)

Show Material materials with Thermal conductivity of 40 W/(m·K)

quenched and tempered (+QT)

EN 10025-6, EN 10137-2

Flat

400 °C

39 W/(m·K)

Show Material materials with Thermal conductivity of 39 W/(m·K)

quenched and tempered (+QT)

EN 10025-6, EN 10137-2

Flat

500 °C

37 W/(m·K)

Show Material materials with Thermal conductivity of 37 W/(m·K)

quenched and tempered (+QT)

EN 10025-6, EN 10137-2

Flat

Electrical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Electrical conductivity

5 S/m

Show Material materials with Electrical conductivity of 5 S/m

Predicted Value

Electrical resistivity

20 °C

2.8e-07 Ω·m

Show Material materials with Electrical resistivity of 2.8e-07 Ω·m

quenched and tempered (+QT)

EN 10025-6, EN 10137-2

Flat

100 °C

3.3e-07 Ω·m

Show Material materials with Electrical resistivity of 3.3e-07 Ω·m

quenched and tempered (+QT)

EN 10025-6, EN 10137-2

Flat

200 °C

3.9e-07 Ω·m

Show Material materials with Electrical resistivity of 3.9e-07 Ω·m

quenched and tempered (+QT)

EN 10025-6, EN 10137-2

Flat

300 °C

4.7e-07 Ω·m

Show Material materials with Electrical resistivity of 4.7e-07 Ω·m

quenched and tempered (+QT)

EN 10025-6, EN 10137-2

Flat

400 °C

5.7e-07 Ω·m

Show Material materials with Electrical resistivity of 5.7e-07 Ω·m

quenched and tempered (+QT)

EN 10025-6, EN 10137-2

Flat

500 °C

6.7e-07 Ω·m

Show Material materials with Electrical resistivity of 6.7e-07 Ω·m

quenched and tempered (+QT)

EN 10025-6, EN 10137-2

Flat

Chemical properties

PropertyValueConditionRelated StandardsShape

Aluminium

0.015 %

Show Material materials with Aluminium of 0.015 %

quenched and tempered (+QT)

EN 10137-2

Sheet, Flat

Boron

0.005 %

Show Material materials with Boron of 0.005 %

quenched and tempered (+QT)

EN 10137-2, EN 10025-6, VdTÜV WB 257

Sheet, Flat

Carbon

0.2 %

Show Material materials with Carbon of 0.2 %

quenched and tempered (+QT)

EN 10137-2, EN 10025-6, VdTÜV WB 257

Sheet, Flat

Chromium

1.5 %

Show Material materials with Chromium of 1.5 %

quenched and tempered (+QT)

EN 10137-2, EN 10025-6, VdTÜV WB 257

Sheet, Flat

Copper

0.5 %

Show Material materials with Copper of 0.5 %

quenched and tempered (+QT)

EN 10137-2, EN 10025-6, VdTÜV WB 257

Sheet, Flat

Manganese

1.6 %

Show Material materials with Manganese of 1.6 %

quenched and tempered (+QT)

EN 10137-2

Sheet, Flat

1.7 %

Show Material materials with Manganese of 1.7 %

quenched and tempered (+QT)

EN 10137-2, EN 10025-6, VdTÜV WB 257

Sheet, Flat

Molybdenum

0.6 %

Show Material materials with Molybdenum of 0.6 %

quenched and tempered (+QT)

EN 10137-2

Sheet, Flat

0.7 %

Show Material materials with Molybdenum of 0.7 %

quenched and tempered (+QT)

EN 10137-2, EN 10025-6, VdTÜV WB 257

Sheet, Flat

Nickel

2 %

Show Material materials with Nickel of 2 %

quenched and tempered (+QT)

EN 10137-2, EN 10025-6, VdTÜV WB 257

Sheet, Flat

Niobium

0.06 %

Show Material materials with Niobium of 0.06 %

quenched and tempered (+QT)

EN 10137-2, EN 10025-6, VdTÜV WB 257

Sheet, Flat

Nitrogen

0.015 %

Show Material materials with Nitrogen of 0.015 %

quenched and tempered (+QT)

EN 10137-2, EN 10025-6, VdTÜV WB 257

Sheet, Flat

Phosphorus

0.02 %

Show Material materials with Phosphorus of 0.02 %

quenched and tempered (+QT)

EN 10137-2, EN 10025-6, VdTÜV WB 257

Sheet, Flat

Silicon

0.8 %

Show Material materials with Silicon of 0.8 %

quenched and tempered (+QT)

EN 10137-2, EN 10025-6, VdTÜV WB 257

Sheet, Flat

Sulfur

0.01 %

Show Material materials with Sulfur of 0.01 %

quenched and tempered (+QT)

EN 10137-2, EN 10025-6, VdTÜV WB 257

Sheet, Flat

Titanium

0.05 %

Show Material materials with Titanium of 0.05 %

quenched and tempered (+QT)

EN 10137-2, EN 10025-6, VdTÜV WB 257

Sheet, Flat

Vanadium

0.12 %

Show Material materials with Vanadium of 0.12 %

quenched and tempered (+QT)

EN 10137-2, EN 10025-6, VdTÜV WB 257

Sheet, Flat

Zirconium

0.12 %

Show Material materials with Zirconium of 0.12 %

quenched and tempered (+QT)

EN 10137-2

Sheet, Flat

0.15 %

Show Material materials with Zirconium of 0.15 %

quenched and tempered (+QT)

EN 10137-2, EN 10025-6, VdTÜV WB 257

Sheet, Flat

Technological properties

Property
Supplier Disclaimer

The given information is a rough description and some properties can depend on various factors such as product thickness. Please contact the supplier or refer to the related norm or standard for further information.

Do you have a technical question or need more information about this material?