General
Property | Value | Temperature |
---|---|---|
Density | 7.88 g/cm³ Show Material materials with Density of 7.88 g/cm³ at 20.0 °C | 20.0 °C |
7.84 g/cm³ Show Material materials with Density of 7.84 g/cm³ at 27.0 °C | 27.0 °C | |
Mechanical
Property | Value | Temperature |
---|---|---|
Elastic modulus | 205.5 GPa Show Material materials with Elastic modulus of 205.5 GPa at -269.0 °C | -269.0 °C |
205.2 GPa Show Material materials with Elastic modulus of 205.2 GPa at -200.0 °C | -200.0 °C | |
203.4 GPa Show Material materials with Elastic modulus of 203.4 GPa at -150.0 °C | -150.0 °C | |
201 - 201.4 GPa Show Material materials with Elastic modulus of 201 - 201.4 GPa at -100.0 °C | -100.0 °C | |
198.9 GPa Show Material materials with Elastic modulus of 198.9 GPa at -50.0 °C | -50.0 °C | |
195 GPa Show Material materials with Elastic modulus of 195 GPa at 20.0 °C | 20.0 °C | |
195.1 GPa Show Material materials with Elastic modulus of 195.1 GPa at 27.0 °C | 27.0 °C | |
190 GPa Show Material materials with Elastic modulus of 190 GPa at 100.0 °C | 100.0 °C | |
184 GPa Show Material materials with Elastic modulus of 184 GPa at 200.0 °C | 200.0 °C | |
178 GPa Show Material materials with Elastic modulus of 178 GPa at 300.0 °C | 300.0 °C | |
170 GPa Show Material materials with Elastic modulus of 170 GPa at 400.0 °C | 400.0 °C | |
Elongation | 18 % Show Material materials with Elongation of 18 % at 20.0 °C | 20.0 °C |
Poisson's ratio | 0.29 [-] Show Material materials with Poisson's ratio of 0.29 [-] at -269.0 °C | -269.0 °C |
0.29 [-] Show Material materials with Poisson's ratio of 0.29 [-] at -200.0 °C | -200.0 °C | |
0.29 [-] Show Material materials with Poisson's ratio of 0.29 [-] at -150.0 °C | -150.0 °C | |
0.29 [-] Show Material materials with Poisson's ratio of 0.29 [-] at -100.0 °C | -100.0 °C | |
0.29 [-] Show Material materials with Poisson's ratio of 0.29 [-] at -50.0 °C | -50.0 °C | |
0.29 [-] Show Material materials with Poisson's ratio of 0.29 [-] at 27.0 °C | 27.0 °C | |
Reduction of area | 50 % Show Material materials with Reduction of area of 50 % at 20.0 °C | 20.0 °C |
Shear modulus | 80 GPa Show Material materials with Shear modulus of 80 GPa at -269.0 °C | -269.0 °C |
79.8 GPa Show Material materials with Shear modulus of 79.8 GPa at -200.0 °C | -200.0 °C | |
79 GPa Show Material materials with Shear modulus of 79 GPa at -150.0 °C | -150.0 °C | |
78.2 GPa Show Material materials with Shear modulus of 78.2 GPa at -100.0 °C | -100.0 °C | |
77.1 GPa Show Material materials with Shear modulus of 77.1 GPa at -50.0 °C | -50.0 °C | |
75.4 GPa Show Material materials with Shear modulus of 75.4 GPa at 27.0 °C | 27.0 °C | |
Tensile strength | 680 - 820 MPa Show Material materials with Tensile strength of 680 - 820 MPa at 20.0 °C | 20.0 °C |
Yield strength Rp0.2 | 575 - 585 MPa Show Material materials with Yield strength Rp0.2 of 575 - 585 MPa at 20.0 °C | 20.0 °C |
Thermal
Property | Value | Temperature | Comment |
---|---|---|---|
Coefficient of thermal expansion | 1.02E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.02E-5 1/K at -100.0 °C | -100.0 °C | |
1.1E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.1E-5 1/K at 20.0 °C | 20.0 °C | ||
1.14E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.14E-5 1/K at 100.0 °C | 100.0 °C | ||
1.18E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.18E-5 1/K at 200.0 °C | 200.0 °C | ||
1.21E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.21E-5 1/K at 300.0 °C | 300.0 °C | ||
1.25E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.25E-5 1/K at 400.0 °C | 400.0 °C | ||
Max service temperature, long | -200 - 0 °C Show Material materials with Max service temperature, long of -200 - 0 °C | ||
Melting point | 1316 - 1595 °C Show Material materials with Melting point of 1316 - 1595 °C | Typical for Nickel Steel | |
Specific heat capacity | 442 J/(kg·K) Show Material materials with Specific heat capacity of 442 J/(kg·K) at -100.0 °C | -100.0 °C | |
464 J/(kg·K) Show Material materials with Specific heat capacity of 464 J/(kg·K) at 20.0 °C | 20.0 °C | ||
479 J/(kg·K) Show Material materials with Specific heat capacity of 479 J/(kg·K) at 100.0 °C | 100.0 °C | ||
495 J/(kg·K) Show Material materials with Specific heat capacity of 495 J/(kg·K) at 200.0 °C | 200.0 °C | ||
511 J/(kg·K) Show Material materials with Specific heat capacity of 511 J/(kg·K) at 300.0 °C | 300.0 °C | ||
528 J/(kg·K) Show Material materials with Specific heat capacity of 528 J/(kg·K) at 400.0 °C | 400.0 °C | ||
Thermal conductivity | 23.9 W/(m·K) Show Material materials with Thermal conductivity of 23.9 W/(m·K) at -100.0 °C | -100.0 °C | |
30.2 W/(m·K) Show Material materials with Thermal conductivity of 30.2 W/(m·K) at 20.0 °C | 20.0 °C | ||
32.8 W/(m·K) Show Material materials with Thermal conductivity of 32.8 W/(m·K) at 100.0 °C | 100.0 °C | ||
34.4 W/(m·K) Show Material materials with Thermal conductivity of 34.4 W/(m·K) at 200.0 °C | 200.0 °C | ||
34.7 W/(m·K) Show Material materials with Thermal conductivity of 34.7 W/(m·K) at 300.0 °C | 300.0 °C | ||
34 W/(m·K) Show Material materials with Thermal conductivity of 34 W/(m·K) at 400.0 °C | 400.0 °C | ||
Thermal diffusivity | 8.3 mm²/s Show Material materials with Thermal diffusivity of 8.3 mm²/s at 20.0 °C | 20.0 °C | |
8.5 mm²/s Show Material materials with Thermal diffusivity of 8.5 mm²/s at 100.0 °C | 100.0 °C | ||
8.4 mm²/s Show Material materials with Thermal diffusivity of 8.4 mm²/s at 200.0 °C | 200.0 °C | ||
8 mm²/s Show Material materials with Thermal diffusivity of 8 mm²/s at 300.0 °C | 300.0 °C | ||
7.3 mm²/s Show Material materials with Thermal diffusivity of 7.3 mm²/s at 400.0 °C | 400.0 °C | ||
Electrical
Property | Value | Temperature |
---|---|---|
Electrical resistivity | 2.51E-7 Ω·m Show Material materials with Electrical resistivity of 2.51E-7 Ω·m at -100.0 °C | -100.0 °C |
3.22E-7 Ω·m Show Material materials with Electrical resistivity of 3.22E-7 Ω·m at 20.0 °C | 20.0 °C | |
3.73E-7 Ω·m Show Material materials with Electrical resistivity of 3.73E-7 Ω·m at 100.0 °C | 100.0 °C | |
4.4E-7 Ω·m Show Material materials with Electrical resistivity of 4.4E-7 Ω·m at 200.0 °C | 200.0 °C | |
5.19E-7 Ω·m Show Material materials with Electrical resistivity of 5.19E-7 Ω·m at 300.0 °C | 300.0 °C | |
6.13E-7 Ω·m Show Material materials with Electrical resistivity of 6.13E-7 Ω·m at 400.0 °C | 400.0 °C | |
Chemical properties
Property | ||
---|---|---|
Carbon | 0.1 % | |
Manganese | 0.3 - 0.8 % | |
Molybdenum | 0.1 % | |
Nickel | 8.5 - 10 % | |
Phosphorus | 0.02 % | |
Silicon | 0.35 % | |
Sulfur | 0.01 % | |
Vanadium | 0.05 % |