EN 10269 Grade X15CrMo5-1 normalized and tempered (+NT)

Want to keep this datasheet? Save it now in your required format

Description

Application for mounting elements at increased temperatures.

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueComment

Density

23.0 °C

7.8 - 7.9 g/cm³

Show Material materials with Density of 7.8 - 7.9 g/cm³

Typical for Chromium Molybdenum Steel

Mechanical

PropertyTemperatureValueComment

Elastic modulus

23.0 °C

200 - 215 GPa

Show Material materials with Elastic modulus of 200 - 215 GPa

Typical for Chromium Molybdenum Steel

Elongation

20.0 °C

14 %

Show Material materials with Elongation of 14 %

Poisson's ratio

23.0 °C

0.29 [-]

Show Material materials with Poisson's ratio of 0.29 [-]

Typical for Chromium Molybdenum Steel

Reduction of area

20.0 °C

45 %

Show Material materials with Reduction of area of 45 %

Tensile strength

20.0 °C

640 - 780 MPa

Show Material materials with Tensile strength of 640 - 780 MPa

Yield strength Rp0.2

20.0 °C

420 MPa

Show Material materials with Yield strength Rp0.2 of 420 MPa

50.0 °C

392 MPa

Show Material materials with Yield strength Rp0.2 of 392 MPa

100.0 °C

345 MPa

Show Material materials with Yield strength Rp0.2 of 345 MPa

150.0 °C

335 MPa

Show Material materials with Yield strength Rp0.2 of 335 MPa

200.0 °C

327 MPa

Show Material materials with Yield strength Rp0.2 of 327 MPa

250.0 °C

323 MPa

Show Material materials with Yield strength Rp0.2 of 323 MPa

300.0 °C

322 MPa

Show Material materials with Yield strength Rp0.2 of 322 MPa

350.0 °C

316 MPa

Show Material materials with Yield strength Rp0.2 of 316 MPa

400.0 °C

306 MPa

Show Material materials with Yield strength Rp0.2 of 306 MPa

450.0 °C

285 MPa

Show Material materials with Yield strength Rp0.2 of 285 MPa

500.0 °C

256 MPa

Show Material materials with Yield strength Rp0.2 of 256 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

23.0 °C

1.1E-5 - 1.4E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.1E-5 - 1.4E-5 1/K

Typical for Chromium Molybdenum Steel

Melting point

1382 - 1529 °C

Show Material materials with Melting point of 1382 - 1529 °C

Typical for Chromium Molybdenum Steel

Specific heat capacity

23.0 °C

448 - 502 J/(kg·K)

Show Material materials with Specific heat capacity of 448 - 502 J/(kg·K)

Typical for Chromium Molybdenum Steel

Thermal conductivity

23.0 °C

36 - 43 W/(m·K)

Show Material materials with Thermal conductivity of 36 - 43 W/(m·K)

Typical for Chromium Molybdenum Steel

Chemical properties

PropertyValue

Carbon

0.18 %

Show Material materials with Carbon of 0.18 %

Chromium

4 - 6 %

Show Material materials with Chromium of 4 - 6 %

Manganese

0.3 - 0.8 %

Show Material materials with Manganese of 0.3 - 0.8 %

Molybdenum

0.45 - 0.65 %

Show Material materials with Molybdenum of 0.45 - 0.65 %

Phosphorus

0.03 %

Show Material materials with Phosphorus of 0.03 %

Silicon

0.4 %

Show Material materials with Silicon of 0.4 %

Sulfur

0.015 %

Show Material materials with Sulfur of 0.015 %