EN 10269 Grade X6CrNi18-10 solution annealed (+AT)

Want to keep this datasheet? Save it now in your required format

Description

The unstabilized austenitic steel X6CrNi18-10 (1.4948) shows good thermal resistance up to 650 °C Application in reactor engineering (sodium cooling circuit at fast breeders) as well as in steam boiler construction and in chemical industry. Further application for mounting elements at increased temperatures.

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

7.9 - 7.93 g/cm³

Show Material materials with Density of 7.9 - 7.93 g/cm³

Mechanical

PropertyTemperatureValueComment

Elastic modulus

-100.0 °C

206 GPa

Show Material materials with Elastic modulus of 206 GPa

20.0 °C

196 - 200 GPa

Show Material materials with Elastic modulus of 196 - 200 GPa

100.0 °C

190 - 194 GPa

Show Material materials with Elastic modulus of 190 - 194 GPa

200.0 °C

182 - 186 GPa

Show Material materials with Elastic modulus of 182 - 186 GPa

300.0 °C

174 - 179 GPa

Show Material materials with Elastic modulus of 174 - 179 GPa

400.0 °C

166 - 172 GPa

Show Material materials with Elastic modulus of 166 - 172 GPa

500.0 °C

158 - 165 GPa

Show Material materials with Elastic modulus of 158 - 165 GPa

600.0 °C

150 GPa

Show Material materials with Elastic modulus of 150 GPa

700.0 °C

142 GPa

Show Material materials with Elastic modulus of 142 GPa

800.0 °C

134 GPa

Show Material materials with Elastic modulus of 134 GPa

900.0 °C

127 GPa

Show Material materials with Elastic modulus of 127 GPa

1000.0 °C

120 GPa

Show Material materials with Elastic modulus of 120 GPa

Elongation

20.0 °C

40 %

Show Material materials with Elongation of 40 %

Poisson's ratio

23.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

Typical for Austenitic Stainless Steel

Shear modulus

23.0 °C

77 GPa

Show Material materials with Shear modulus of 77 GPa

Typical for Austenitic Stainless Steel

Tensile strength

20.0 °C

500 - 700 MPa

Show Material materials with Tensile strength of 500 - 700 MPa

50.0 °C

480 MPa

Show Material materials with Tensile strength of 480 MPa

100.0 °C

450 MPa

Show Material materials with Tensile strength of 450 MPa

150.0 °C

420 MPa

Show Material materials with Tensile strength of 420 MPa

200.0 °C

400 MPa

Show Material materials with Tensile strength of 400 MPa

250.0 °C

390 MPa

Show Material materials with Tensile strength of 390 MPa

300.0 °C

380 MPa

Show Material materials with Tensile strength of 380 MPa

350.0 °C

380 MPa

Show Material materials with Tensile strength of 380 MPa

400.0 °C

380 MPa

Show Material materials with Tensile strength of 380 MPa

450.0 °C

375 MPa

Show Material materials with Tensile strength of 375 MPa

500.0 °C

360 MPa

Show Material materials with Tensile strength of 360 MPa

550.0 °C

335 MPa

Show Material materials with Tensile strength of 335 MPa

600.0 °C

300 MPa

Show Material materials with Tensile strength of 300 MPa

Unlock all property charts

Yield strength Rp0.2

20.0 °C

185 MPa

Show Material materials with Yield strength Rp0.2 of 185 MPa

50.0 °C

174 MPa

Show Material materials with Yield strength Rp0.2 of 174 MPa

100.0 °C

157 MPa

Show Material materials with Yield strength Rp0.2 of 157 MPa

150.0 °C

142 MPa

Show Material materials with Yield strength Rp0.2 of 142 MPa

200.0 °C

127 MPa

Show Material materials with Yield strength Rp0.2 of 127 MPa

250.0 °C

117 MPa

Show Material materials with Yield strength Rp0.2 of 117 MPa

300.0 °C

108 MPa

Show Material materials with Yield strength Rp0.2 of 108 MPa

350.0 °C

103 MPa

Show Material materials with Yield strength Rp0.2 of 103 MPa

400.0 °C

98 MPa

Show Material materials with Yield strength Rp0.2 of 98 MPa

450.0 °C

93 MPa

Show Material materials with Yield strength Rp0.2 of 93 MPa

500.0 °C

88 MPa

Show Material materials with Yield strength Rp0.2 of 88 MPa

550.0 °C

83 MPa

Show Material materials with Yield strength Rp0.2 of 83 MPa

600.0 °C

78 MPa

Show Material materials with Yield strength Rp0.2 of 78 MPa

Unlock all property charts

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

-100.0 °C

1.49E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.49E-5 1/K

20.0 °C

1.61E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.61E-5 1/K

100.0 °C

1.63E-5 - 1.67E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.63E-5 - 1.67E-5 1/K

200.0 °C

1.69E-5 - 1.72E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.69E-5 - 1.72E-5 1/K

300.0 °C

1.73E-5 - 1.77E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.73E-5 - 1.77E-5 1/K

400.0 °C

1.76E-5 - 1.81E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.76E-5 - 1.81E-5 1/K

500.0 °C

1.82E-5 - 1.84E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.82E-5 - 1.84E-5 1/K

600.0 °C

1.85E-5 - 1.88E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.85E-5 - 1.88E-5 1/K

700.0 °C

1.91E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.91E-5 1/K

800.0 °C

1.94E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.94E-5 1/K

900.0 °C

1.97E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.97E-5 1/K

1000.0 °C

2E-5 1/K

Show Material materials with Coefficient of thermal expansion of 2E-5 1/K

Unlock all property charts

Max service temperature, long

0 - 750 °C

Show Material materials with Max service temperature, long of 0 - 750 °C

Melting point

1230 - 1480 °C

Show Material materials with Melting point of 1230 - 1480 °C

Typical for Austenitic Stainless Steel

Specific heat capacity

-100.0 °C

440 J/(kg·K)

Show Material materials with Specific heat capacity of 440 J/(kg·K)

20.0 °C

450 - 472 J/(kg·K)

Show Material materials with Specific heat capacity of 450 - 472 J/(kg·K)

100.0 °C

487 J/(kg·K)

Show Material materials with Specific heat capacity of 487 J/(kg·K)

200.0 °C

503 J/(kg·K)

Show Material materials with Specific heat capacity of 503 J/(kg·K)

300.0 °C

512 J/(kg·K)

Show Material materials with Specific heat capacity of 512 J/(kg·K)

400.0 °C

520 J/(kg·K)

Show Material materials with Specific heat capacity of 520 J/(kg·K)

500.0 °C

530 J/(kg·K)

Show Material materials with Specific heat capacity of 530 J/(kg·K)

600.0 °C

541 J/(kg·K)

Show Material materials with Specific heat capacity of 541 J/(kg·K)

700.0 °C

551 J/(kg·K)

Show Material materials with Specific heat capacity of 551 J/(kg·K)

800.0 °C

559 J/(kg·K)

Show Material materials with Specific heat capacity of 559 J/(kg·K)

900.0 °C

565 J/(kg·K)

Show Material materials with Specific heat capacity of 565 J/(kg·K)

1000.0 °C

571 J/(kg·K)

Show Material materials with Specific heat capacity of 571 J/(kg·K)

Unlock all property charts

Thermal conductivity

20.0 °C

14.3 - 16 W/(m·K)

Show Material materials with Thermal conductivity of 14.3 - 16 W/(m·K)

100.0 °C

15.8 W/(m·K)

Show Material materials with Thermal conductivity of 15.8 W/(m·K)

200.0 °C

17.5 W/(m·K)

Show Material materials with Thermal conductivity of 17.5 W/(m·K)

300.0 °C

19 W/(m·K)

Show Material materials with Thermal conductivity of 19 W/(m·K)

400.0 °C

20.5 W/(m·K)

Show Material materials with Thermal conductivity of 20.5 W/(m·K)

500.0 °C

21.9 W/(m·K)

Show Material materials with Thermal conductivity of 21.9 W/(m·K)

600.0 °C

23.3 W/(m·K)

Show Material materials with Thermal conductivity of 23.3 W/(m·K)

700.0 °C

24.6 W/(m·K)

Show Material materials with Thermal conductivity of 24.6 W/(m·K)

800.0 °C

26 W/(m·K)

Show Material materials with Thermal conductivity of 26 W/(m·K)

900.0 °C

27.4 W/(m·K)

Show Material materials with Thermal conductivity of 27.4 W/(m·K)

1000.0 °C

28.8 W/(m·K)

Show Material materials with Thermal conductivity of 28.8 W/(m·K)

Unlock all property charts

Thermal diffusivity

20.0 °C

3.8 mm²/s

Show Material materials with Thermal diffusivity of 3.8 mm²/s

100.0 °C

4 mm²/s

Show Material materials with Thermal diffusivity of 4 mm²/s

200.0 °C

4.2 mm²/s

Show Material materials with Thermal diffusivity of 4.2 mm²/s

300.0 °C

4.6 mm²/s

Show Material materials with Thermal diffusivity of 4.6 mm²/s

400.0 °C

4.8 mm²/s

Show Material materials with Thermal diffusivity of 4.8 mm²/s

500.0 °C

4.9 mm²/s

Show Material materials with Thermal diffusivity of 4.9 mm²/s

600.0 °C

5 mm²/s

Show Material materials with Thermal diffusivity of 5 mm²/s

700.0 °C

5.3 mm²/s

Show Material materials with Thermal diffusivity of 5.3 mm²/s

800.0 °C

5.6 mm²/s

Show Material materials with Thermal diffusivity of 5.6 mm²/s

900.0 °C

5.9 mm²/s

Show Material materials with Thermal diffusivity of 5.9 mm²/s

1000.0 °C

6 mm²/s

Show Material materials with Thermal diffusivity of 6 mm²/s

Unlock all property charts

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

7.1E-7 Ω·m

Show Material materials with Electrical resistivity of 7.1E-7 Ω·m

100.0 °C

7.76E-7 Ω·m

Show Material materials with Electrical resistivity of 7.76E-7 Ω·m

200.0 °C

8.49E-7 Ω·m

Show Material materials with Electrical resistivity of 8.49E-7 Ω·m

300.0 °C

9.14E-7 Ω·m

Show Material materials with Electrical resistivity of 9.14E-7 Ω·m

400.0 °C

9.71E-7 Ω·m

Show Material materials with Electrical resistivity of 9.71E-7 Ω·m

500.0 °C

1.02E-6 Ω·m

Show Material materials with Electrical resistivity of 1.02E-6 Ω·m

600.0 °C

1.07E-6 Ω·m

Show Material materials with Electrical resistivity of 1.07E-6 Ω·m

700.0 °C

1.1E-6 Ω·m

Show Material materials with Electrical resistivity of 1.1E-6 Ω·m

800.0 °C

1.14E-6 Ω·m

Show Material materials with Electrical resistivity of 1.14E-6 Ω·m

900.0 °C

1.17E-6 Ω·m

Show Material materials with Electrical resistivity of 1.17E-6 Ω·m

1000.0 °C

1.19E-6 Ω·m

Show Material materials with Electrical resistivity of 1.19E-6 Ω·m

Unlock all property charts

Chemical properties

PropertyValue

Carbon

0.04 - 0.08 %

Show Material materials with Carbon of 0.04 - 0.08 %

Chromium

17 - 19 %

Show Material materials with Chromium of 17 - 19 %

Manganese

2 %

Show Material materials with Manganese of 2 %

Nickel

8 - 11 %

Show Material materials with Nickel of 8 - 11 %

Nitrogen

0.1 - 0.11 %

Show Material materials with Nitrogen of 0.1 - 0.11 %

Phosphorus

0.04 %

Show Material materials with Phosphorus of 0.04 %

Silicon

1 %

Show Material materials with Silicon of 1 %

Sulfur

0.015 %

Show Material materials with Sulfur of 0.015 %