EN 10269 Grade X3CrNiMoBN17-13-3 solution annealed (+AT)

Want to keep this datasheet? Save it now in your required format

Description

N-alloyed steel for application in power station engineering, for superheater and superheated steam conduits, headers, heat exchangers and other high-stress components. Application temperature in continuous operation: 800 °C The steel is insensitive to hot cracks (after welding). Further application for mounting elements at increased temperatures.

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

7.98 - 8 g/cm³

Show Material materials with Density of 7.98 - 8 g/cm³

Mechanical

PropertyTemperatureValueComment

Elastic modulus

-100.0 °C

206 GPa

Show Material materials with Elastic modulus of 206 GPa

20.0 °C

196 - 198 GPa

Show Material materials with Elastic modulus of 196 - 198 GPa

100.0 °C

190 - 192 GPa

Show Material materials with Elastic modulus of 190 - 192 GPa

200.0 °C

182 - 183 GPa

Show Material materials with Elastic modulus of 182 - 183 GPa

300.0 °C

174 - 175 GPa

Show Material materials with Elastic modulus of 174 - 175 GPa

400.0 °C

166 - 167 GPa

Show Material materials with Elastic modulus of 166 - 167 GPa

500.0 °C

158 - 159 GPa

Show Material materials with Elastic modulus of 158 - 159 GPa

600.0 °C

150 GPa

Show Material materials with Elastic modulus of 150 GPa

700.0 °C

142 GPa

Show Material materials with Elastic modulus of 142 GPa

800.0 °C

134 GPa

Show Material materials with Elastic modulus of 134 GPa

900.0 °C

127 GPa

Show Material materials with Elastic modulus of 127 GPa

1000.0 °C

120 GPa

Show Material materials with Elastic modulus of 120 GPa

Elongation

20.0 °C

35 %

Show Material materials with Elongation of 35 %

Poisson's ratio

23.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

Typical for Austenitic Stainless Steel

Shear modulus

23.0 °C

77 GPa

Show Material materials with Shear modulus of 77 GPa

Typical for Austenitic Stainless Steel

Tensile strength

20.0 °C

550 - 750 MPa

Show Material materials with Tensile strength of 550 - 750 MPa

50.0 °C

550 MPa

Show Material materials with Tensile strength of 550 MPa

100.0 °C

520 MPa

Show Material materials with Tensile strength of 520 MPa

150.0 °C

490 MPa

Show Material materials with Tensile strength of 490 MPa

200.0 °C

460 MPa

Show Material materials with Tensile strength of 460 MPa

250.0 °C

450 MPa

Show Material materials with Tensile strength of 450 MPa

300.0 °C

440 MPa

Show Material materials with Tensile strength of 440 MPa

350.0 °C

435 MPa

Show Material materials with Tensile strength of 435 MPa

400.0 °C

435 MPa

Show Material materials with Tensile strength of 435 MPa

450.0 °C

435 MPa

Show Material materials with Tensile strength of 435 MPa

500.0 °C

430 MPa

Show Material materials with Tensile strength of 430 MPa

550.0 °C

410 MPa

Show Material materials with Tensile strength of 410 MPa

600.0 °C

380 MPa

Show Material materials with Tensile strength of 380 MPa

Unlock all property charts

Yield strength Rp0.2

20.0 °C

260 MPa

Show Material materials with Yield strength Rp0.2 of 260 MPa

50.0 °C

239 MPa

Show Material materials with Yield strength Rp0.2 of 239 MPa

100.0 °C

205 MPa

Show Material materials with Yield strength Rp0.2 of 205 MPa

150.0 °C

187 MPa

Show Material materials with Yield strength Rp0.2 of 187 MPa

200.0 °C

170 MPa

Show Material materials with Yield strength Rp0.2 of 170 MPa

250.0 °C

159 MPa

Show Material materials with Yield strength Rp0.2 of 159 MPa

300.0 °C

148 MPa

Show Material materials with Yield strength Rp0.2 of 148 MPa

350.0 °C

141 MPa

Show Material materials with Yield strength Rp0.2 of 141 MPa

400.0 °C

134 MPa

Show Material materials with Yield strength Rp0.2 of 134 MPa

450.0 °C

130 MPa

Show Material materials with Yield strength Rp0.2 of 130 MPa

500.0 °C

127 MPa

Show Material materials with Yield strength Rp0.2 of 127 MPa

550.0 °C

124 MPa

Show Material materials with Yield strength Rp0.2 of 124 MPa

600.0 °C

121 MPa

Show Material materials with Yield strength Rp0.2 of 121 MPa

Unlock all property charts

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

-100.0 °C

1.49E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.49E-5 1/K

20.0 °C

1.61E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.61E-5 1/K

100.0 °C

1.63E-5 - 1.67E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.63E-5 - 1.67E-5 1/K

200.0 °C

1.68E-5 - 1.72E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.68E-5 - 1.72E-5 1/K

300.0 °C

1.73E-5 - 1.77E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.73E-5 - 1.77E-5 1/K

400.0 °C

1.76E-5 - 1.81E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.76E-5 - 1.81E-5 1/K

500.0 °C

1.82E-5 - 1.84E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.82E-5 - 1.84E-5 1/K

600.0 °C

1.85E-5 - 1.88E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.85E-5 - 1.88E-5 1/K

700.0 °C

1.91E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.91E-5 1/K

800.0 °C

1.94E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.94E-5 1/K

900.0 °C

1.97E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.97E-5 1/K

1000.0 °C

2E-5 1/K

Show Material materials with Coefficient of thermal expansion of 2E-5 1/K

Unlock all property charts

Max service temperature, long

600 - 800 °C

Show Material materials with Max service temperature, long of 600 - 800 °C

Melting point

1230 - 1480 °C

Show Material materials with Melting point of 1230 - 1480 °C

Typical for Austenitic Stainless Steel

Specific heat capacity

-100.0 °C

440 J/(kg·K)

Show Material materials with Specific heat capacity of 440 J/(kg·K)

20.0 °C

450 - 472 J/(kg·K)

Show Material materials with Specific heat capacity of 450 - 472 J/(kg·K)

100.0 °C

487 J/(kg·K)

Show Material materials with Specific heat capacity of 487 J/(kg·K)

200.0 °C

503 J/(kg·K)

Show Material materials with Specific heat capacity of 503 J/(kg·K)

300.0 °C

512 J/(kg·K)

Show Material materials with Specific heat capacity of 512 J/(kg·K)

400.0 °C

520 J/(kg·K)

Show Material materials with Specific heat capacity of 520 J/(kg·K)

500.0 °C

530 J/(kg·K)

Show Material materials with Specific heat capacity of 530 J/(kg·K)

600.0 °C

541 J/(kg·K)

Show Material materials with Specific heat capacity of 541 J/(kg·K)

700.0 °C

551 J/(kg·K)

Show Material materials with Specific heat capacity of 551 J/(kg·K)

800.0 °C

559 J/(kg·K)

Show Material materials with Specific heat capacity of 559 J/(kg·K)

900.0 °C

565 J/(kg·K)

Show Material materials with Specific heat capacity of 565 J/(kg·K)

1000.0 °C

571 J/(kg·K)

Show Material materials with Specific heat capacity of 571 J/(kg·K)

Unlock all property charts

Thermal conductivity

20.0 °C

13.5 - 16 W/(m·K)

Show Material materials with Thermal conductivity of 13.5 - 16 W/(m·K)

100.0 °C

15 W/(m·K)

Show Material materials with Thermal conductivity of 15 W/(m·K)

200.0 °C

16.7 W/(m·K)

Show Material materials with Thermal conductivity of 16.7 W/(m·K)

300.0 °C

18.3 W/(m·K)

Show Material materials with Thermal conductivity of 18.3 W/(m·K)

400.0 °C

19.8 W/(m·K)

Show Material materials with Thermal conductivity of 19.8 W/(m·K)

500.0 °C

21.2 W/(m·K)

Show Material materials with Thermal conductivity of 21.2 W/(m·K)

600.0 °C

22.7 W/(m·K)

Show Material materials with Thermal conductivity of 22.7 W/(m·K)

700.0 °C

24.1 W/(m·K)

Show Material materials with Thermal conductivity of 24.1 W/(m·K)

800.0 °C

25.5 W/(m·K)

Show Material materials with Thermal conductivity of 25.5 W/(m·K)

900.0 °C

26.9 W/(m·K)

Show Material materials with Thermal conductivity of 26.9 W/(m·K)

1000.0 °C

28.3 W/(m·K)

Show Material materials with Thermal conductivity of 28.3 W/(m·K)

Unlock all property charts

Thermal diffusivity

20.0 °C

3.6 mm²/s

Show Material materials with Thermal diffusivity of 3.6 mm²/s

100.0 °C

3.8 mm²/s

Show Material materials with Thermal diffusivity of 3.8 mm²/s

200.0 °C

4 mm²/s

Show Material materials with Thermal diffusivity of 4 mm²/s

300.0 °C

4.4 mm²/s

Show Material materials with Thermal diffusivity of 4.4 mm²/s

400.0 °C

4.6 mm²/s

Show Material materials with Thermal diffusivity of 4.6 mm²/s

500.0 °C

4.7 mm²/s

Show Material materials with Thermal diffusivity of 4.7 mm²/s

600.0 °C

4.9 mm²/s

Show Material materials with Thermal diffusivity of 4.9 mm²/s

700.0 °C

5.2 mm²/s

Show Material materials with Thermal diffusivity of 5.2 mm²/s

800.0 °C

5.5 mm²/s

Show Material materials with Thermal diffusivity of 5.5 mm²/s

900.0 °C

5.8 mm²/s

Show Material materials with Thermal diffusivity of 5.8 mm²/s

1000.0 °C

5.9 mm²/s

Show Material materials with Thermal diffusivity of 5.9 mm²/s

Unlock all property charts

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

7.7E-7 Ω·m

Show Material materials with Electrical resistivity of 7.7E-7 Ω·m

100.0 °C

8.34E-7 Ω·m

Show Material materials with Electrical resistivity of 8.34E-7 Ω·m

200.0 °C

9.03E-7 Ω·m

Show Material materials with Electrical resistivity of 9.03E-7 Ω·m

300.0 °C

9.64E-7 Ω·m

Show Material materials with Electrical resistivity of 9.64E-7 Ω·m

400.0 °C

1.02E-6 Ω·m

Show Material materials with Electrical resistivity of 1.02E-6 Ω·m

500.0 °C

1.06E-6 Ω·m

Show Material materials with Electrical resistivity of 1.06E-6 Ω·m

600.0 °C

1.1E-6 Ω·m

Show Material materials with Electrical resistivity of 1.1E-6 Ω·m

700.0 °C

1.13E-6 Ω·m

Show Material materials with Electrical resistivity of 1.13E-6 Ω·m

800.0 °C

1.17E-6 Ω·m

Show Material materials with Electrical resistivity of 1.17E-6 Ω·m

900.0 °C

1.19E-6 Ω·m

Show Material materials with Electrical resistivity of 1.19E-6 Ω·m

1000.0 °C

1.22E-6 Ω·m

Show Material materials with Electrical resistivity of 1.22E-6 Ω·m

Unlock all property charts

Chemical properties

PropertyValue

Boron

1.5E-3 - 5E-3 %

Show Material materials with Boron of 1.5E-3 - 5E-3 %

Carbon

0.04 %

Show Material materials with Carbon of 0.04 %

Chromium

16 - 18 %

Show Material materials with Chromium of 16 - 18 %

Manganese

2 %

Show Material materials with Manganese of 2 %

Molybdenum

2 - 3 %

Show Material materials with Molybdenum of 2 - 3 %

Nickel

12 - 14 %

Show Material materials with Nickel of 12 - 14 %

Nitrogen

0.1 - 0.18 %

Show Material materials with Nitrogen of 0.1 - 0.18 %

Phosphorus

0.04 %

Show Material materials with Phosphorus of 0.04 %

Silicon

0.75 %

Show Material materials with Silicon of 0.75 %

Sulfur

0.015 %

Show Material materials with Sulfur of 0.015 %