General
Property | Temperature | Value |
---|---|---|
Density | 20.0 °C | 7.7 - 7.77 g/cm³ Show Material materials with Density of 7.7 - 7.77 g/cm³ |
Mechanical
Property | Temperature | Value |
---|---|---|
Elastic modulus | 20.0 °C | 211.67 - 220 GPa Show Material materials with Elastic modulus of 211.67 - 220 GPa |
100.0 °C | 213 - 215 GPa Show Material materials with Elastic modulus of 213 - 215 GPa | |
200.0 °C | 206 - 210 GPa Show Material materials with Elastic modulus of 206 - 210 GPa | |
300.0 °C | 198 - 205 GPa Show Material materials with Elastic modulus of 198 - 205 GPa | |
400.0 °C | 190 - 195 GPa Show Material materials with Elastic modulus of 190 - 195 GPa | |
500.0 °C | 180 GPa Show Material materials with Elastic modulus of 180 GPa | |
600.0 °C | 167 GPa Show Material materials with Elastic modulus of 167 GPa | |
700.0 °C | 150 GPa Show Material materials with Elastic modulus of 150 GPa | |
Poisson's ratio | 20.0 °C | 0.3 [-] Show Material materials with Poisson's ratio of 0.3 [-] |
Shear modulus | 20.0 °C | 81.7 GPa Show Material materials with Shear modulus of 81.7 GPa |
Yield strength Rp0.2 | 50.0 °C | 265 MPa Show Material materials with Yield strength Rp0.2 of 265 MPa |
100.0 °C | 240 MPa Show Material materials with Yield strength Rp0.2 of 240 MPa | |
150.0 °C | 235 MPa Show Material materials with Yield strength Rp0.2 of 235 MPa | |
200.0 °C | 230 MPa Show Material materials with Yield strength Rp0.2 of 230 MPa | |
250.0 °C | 220 MPa Show Material materials with Yield strength Rp0.2 of 220 MPa | |
300.0 °C | 215 MPa Show Material materials with Yield strength Rp0.2 of 215 MPa | |
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of thermal expansion | -100.0 °C | 1E-5 1/K Show Material materials with Coefficient of thermal expansion of 1E-5 1/K | |
20.0 °C | 1.08E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.08E-5 1/K | ||
100.0 °C | 1.04E-5 - 1.13E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.04E-5 - 1.13E-5 1/K | ||
200.0 °C | 1.08E-5 - 1.18E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.08E-5 - 1.18E-5 1/K | ||
300.0 °C | 1.12E-5 - 1.23E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.12E-5 - 1.23E-5 1/K | ||
400.0 °C | 1.16E-5 - 1.27E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.16E-5 - 1.27E-5 1/K | ||
500.0 °C | 1.19E-5 - 1.3E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.19E-5 - 1.3E-5 1/K | ||
600.0 °C | 1.32E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.32E-5 1/K | ||
700.0 °C | 1.33E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.33E-5 1/K | ||
Melting point | 1425 - 1530 °C Show Material materials with Melting point of 1425 - 1530 °C | Typical for Ferritic Stainless Steel | |
Specific heat capacity | 20.0 °C | 429 - 430 J/(kg·K) Show Material materials with Specific heat capacity of 429 - 430 J/(kg·K) | |
100.0 °C | 464 J/(kg·K) Show Material materials with Specific heat capacity of 464 J/(kg·K) | ||
200.0 °C | 492 J/(kg·K) Show Material materials with Specific heat capacity of 492 J/(kg·K) | ||
300.0 °C | 511 J/(kg·K) Show Material materials with Specific heat capacity of 511 J/(kg·K) | ||
400.0 °C | 531 J/(kg·K) Show Material materials with Specific heat capacity of 531 J/(kg·K) | ||
500.0 °C | 554 J/(kg·K) Show Material materials with Specific heat capacity of 554 J/(kg·K) | ||
600.0 °C | 585 J/(kg·K) Show Material materials with Specific heat capacity of 585 J/(kg·K) | ||
700.0 °C | 626 J/(kg·K) Show Material materials with Specific heat capacity of 626 J/(kg·K) | ||
Thermal conductivity | 20.0 °C | 20.7 - 25 W/(m·K) Show Material materials with Thermal conductivity of 20.7 - 25 W/(m·K) | |
100.0 °C | 22.6 W/(m·K) Show Material materials with Thermal conductivity of 22.6 W/(m·K) | ||
200.0 °C | 24.4 W/(m·K) Show Material materials with Thermal conductivity of 24.4 W/(m·K) | ||
300.0 °C | 25.8 W/(m·K) Show Material materials with Thermal conductivity of 25.8 W/(m·K) | ||
400.0 °C | 26.9 W/(m·K) Show Material materials with Thermal conductivity of 26.9 W/(m·K) | ||
500.0 °C | 27.8 W/(m·K) Show Material materials with Thermal conductivity of 27.8 W/(m·K) | ||
600.0 °C | 28.5 W/(m·K) Show Material materials with Thermal conductivity of 28.5 W/(m·K) | ||
700.0 °C | 28.8 W/(m·K) Show Material materials with Thermal conductivity of 28.8 W/(m·K) | ||
Thermal diffusivity | 20.0 °C | 6.2 mm²/s Show Material materials with Thermal diffusivity of 6.2 mm²/s | |
100.0 °C | 5.9 mm²/s Show Material materials with Thermal diffusivity of 5.9 mm²/s | ||
200.0 °C | 6 mm²/s Show Material materials with Thermal diffusivity of 6 mm²/s | ||
300.0 °C | 6 mm²/s Show Material materials with Thermal diffusivity of 6 mm²/s | ||
400.0 °C | 5.7 mm²/s Show Material materials with Thermal diffusivity of 5.7 mm²/s | ||
500.0 °C | 5.4 mm²/s Show Material materials with Thermal diffusivity of 5.4 mm²/s | ||
600.0 °C | 4.8 mm²/s Show Material materials with Thermal diffusivity of 4.8 mm²/s | ||
700.0 °C | 4 mm²/s Show Material materials with Thermal diffusivity of 4 mm²/s | ||
Electrical
Property | Temperature | Value |
---|---|---|
Electrical resistivity | 20.0 °C | 5.03E-7 - 6E-7 Ω·m Show Material materials with Electrical resistivity of 5.03E-7 - 6E-7 Ω·m |
100.0 °C | 5.67E-7 Ω·m Show Material materials with Electrical resistivity of 5.67E-7 Ω·m | |
200.0 °C | 6.47E-7 Ω·m Show Material materials with Electrical resistivity of 6.47E-7 Ω·m | |
300.0 °C | 7.27E-7 Ω·m Show Material materials with Electrical resistivity of 7.27E-7 Ω·m | |
400.0 °C | 8.09E-7 Ω·m Show Material materials with Electrical resistivity of 8.09E-7 Ω·m | |
500.0 °C | 8.9E-7 Ω·m Show Material materials with Electrical resistivity of 8.9E-7 Ω·m | |
600.0 °C | 9.72E-7 Ω·m Show Material materials with Electrical resistivity of 9.72E-7 Ω·m | |
700.0 °C | 1.06E-6 Ω·m Show Material materials with Electrical resistivity of 1.06E-6 Ω·m | |
Chemical properties
Property | Value |
---|---|
Carbon | 0.03 % Show Material materials with Carbon of 0.03 % |
Chromium | 10.5 - 12.5 % Show Material materials with Chromium of 10.5 - 12.5 % |
Manganese | 1.5 % Show Material materials with Manganese of 1.5 % |
Nickel | 0.3 - 1 % Show Material materials with Nickel of 0.3 - 1 % |
Nitrogen | 0.03 % Show Material materials with Nitrogen of 0.03 % |
Phosphorus | 0.04 % Show Material materials with Phosphorus of 0.04 % |
Silicon | 1 % Show Material materials with Silicon of 1 % |
Sulfur | 0.015 % Show Material materials with Sulfur of 0.015 % |
Do you have a technical question or need more information about this material?