EN 10028-7 Grade X5CrNiN19-9 solution annealed (+AT)

Want to keep this datasheet? Save it now in your required format

Description

The austenitic steel X5CrNiN19-9 is resistant to intercrystalline corrosion in the delivery condition, in welded condition the dimension limits of resistance can vary according to chemical composition and welding conditions. Application: tank construction

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

7.9 g/cm³

Show Material materials with Density of 7.9 g/cm³

Mechanical

PropertyTemperatureValueComment

Elastic modulus

20.0 °C

200 GPa

Show Material materials with Elastic modulus of 200 GPa

100.0 °C

194 - 195 GPa

Show Material materials with Elastic modulus of 194 - 195 GPa

200.0 °C

185 - 186 GPa

Show Material materials with Elastic modulus of 185 - 186 GPa

300.0 °C

179 - 180 GPa

Show Material materials with Elastic modulus of 179 - 180 GPa

400.0 °C

172 GPa

Show Material materials with Elastic modulus of 172 GPa

500.0 °C

165 GPa

Show Material materials with Elastic modulus of 165 GPa

Elongation

-196.0 °C

35 %

Show Material materials with Elongation of 35 %

-150.0 °C

35 %

Show Material materials with Elongation of 35 %

-80.0 °C

40 %

Show Material materials with Elongation of 40 %

20.0 °C

40 %

Show Material materials with Elongation of 40 %

Unlock all property charts

Elongation A80, transverse

20.0 °C

40 %

Show Material materials with Elongation A80, transverse of 40 %

Elongation, transverse

20.0 °C

40 %

Show Material materials with Elongation, transverse of 40 %

Poisson's ratio

23.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

Typical for Ferritic Stainless Steel

Shear modulus

23.0 °C

77 GPa

Show Material materials with Shear modulus of 77 GPa

Typical for Ferritic Stainless Steel

Tensile strength

-196.0 °C

1350 MPa

Show Material materials with Tensile strength of 1350 MPa

-150.0 °C

1180 MPa

Show Material materials with Tensile strength of 1180 MPa

-80.0 °C

890 MPa

Show Material materials with Tensile strength of 890 MPa

20.0 °C

550 - 750 MPa

Show Material materials with Tensile strength of 550 - 750 MPa

50.0 °C

527 MPa

Show Material materials with Tensile strength of 527 MPa

100.0 °C

490 MPa

Show Material materials with Tensile strength of 490 MPa

150.0 °C

460 MPa

Show Material materials with Tensile strength of 460 MPa

200.0 °C

430 MPa

Show Material materials with Tensile strength of 430 MPa

250.0 °C

420 MPa

Show Material materials with Tensile strength of 420 MPa

300.0 °C

410 MPa

Show Material materials with Tensile strength of 410 MPa

350.0 °C

410 MPa

Show Material materials with Tensile strength of 410 MPa

Unlock all property charts

Tensile strength, transverse

20.0 °C

550 - 750 MPa

Show Material materials with Tensile strength, transverse of 550 - 750 MPa

Yield strength Rp0.2

-196.0 °C

550 MPa

Show Material materials with Yield strength Rp0.2 of 550 MPa

-150.0 °C

450 MPa

Show Material materials with Yield strength Rp0.2 of 450 MPa

-80.0 °C

385 MPa

Show Material materials with Yield strength Rp0.2 of 385 MPa

20.0 °C

270 MPa

Show Material materials with Yield strength Rp0.2 of 270 MPa

50.0 °C

246 MPa

Show Material materials with Yield strength Rp0.2 of 246 MPa

100.0 °C

205 MPa

Show Material materials with Yield strength Rp0.2 of 205 MPa

150.0 °C

175 MPa

Show Material materials with Yield strength Rp0.2 of 175 MPa

200.0 °C

157 MPa

Show Material materials with Yield strength Rp0.2 of 157 MPa

250.0 °C

145 MPa

Show Material materials with Yield strength Rp0.2 of 145 MPa

300.0 °C

136 MPa

Show Material materials with Yield strength Rp0.2 of 136 MPa

350.0 °C

130 MPa

Show Material materials with Yield strength Rp0.2 of 130 MPa

400.0 °C

125 MPa

Show Material materials with Yield strength Rp0.2 of 125 MPa

450.0 °C

121 MPa

Show Material materials with Yield strength Rp0.2 of 121 MPa

500.0 °C

119 MPa

Show Material materials with Yield strength Rp0.2 of 119 MPa

550.0 °C

118 MPa

Show Material materials with Yield strength Rp0.2 of 118 MPa

Unlock all property charts

Yield strength Rp0.2, transverse

20.0 °C

270 - 290 MPa

Show Material materials with Yield strength Rp0.2, transverse of 270 - 290 MPa

Yield strength Rp1.0

-196.0 °C

650 MPa

Show Material materials with Yield strength Rp1.0 of 650 MPa

-150.0 °C

550 MPa

Show Material materials with Yield strength Rp1.0 of 550 MPa

-80.0 °C

455 MPa

Show Material materials with Yield strength Rp1.0 of 455 MPa

20.0 °C

310 MPa

Show Material materials with Yield strength Rp1.0 of 310 MPa

50.0 °C

284 MPa

Show Material materials with Yield strength Rp1.0 of 284 MPa

100.0 °C

240 MPa

Show Material materials with Yield strength Rp1.0 of 240 MPa

150.0 °C

210 MPa

Show Material materials with Yield strength Rp1.0 of 210 MPa

200.0 °C

187 MPa

Show Material materials with Yield strength Rp1.0 of 187 MPa

250.0 °C

175 MPa

Show Material materials with Yield strength Rp1.0 of 175 MPa

300.0 °C

167 MPa

Show Material materials with Yield strength Rp1.0 of 167 MPa

350.0 °C

161 MPa

Show Material materials with Yield strength Rp1.0 of 161 MPa

400.0 °C

156 MPa

Show Material materials with Yield strength Rp1.0 of 156 MPa

450.0 °C

152 MPa

Show Material materials with Yield strength Rp1.0 of 152 MPa

500.0 °C

149 MPa

Show Material materials with Yield strength Rp1.0 of 149 MPa

550.0 °C

147 MPa

Show Material materials with Yield strength Rp1.0 of 147 MPa

Unlock all property charts

Yield strength Rp1.0, transverse

20.0 °C

310 - 320 MPa

Show Material materials with Yield strength Rp1.0, transverse of 310 - 320 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

100.0 °C

1.6E-5 - 1.7E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.6E-5 - 1.7E-5 1/K

200.0 °C

1.65E-5 - 1.75E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.65E-5 - 1.75E-5 1/K

300.0 °C

1.7E-5 - 1.8E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.7E-5 - 1.8E-5 1/K

400.0 °C

1.75E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.75E-5 1/K

500.0 °C

1.8E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.8E-5 1/K

Unlock all property charts

Melting point

1425 - 1530 °C

Show Material materials with Melting point of 1425 - 1530 °C

Typical for Ferritic Stainless Steel

Specific heat capacity

20.0 °C

500 J/(kg·K)

Show Material materials with Specific heat capacity of 500 J/(kg·K)

Thermal conductivity

20.0 °C

15 W/(m·K)

Show Material materials with Thermal conductivity of 15 W/(m·K)

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

7.3E-7 Ω·m

Show Material materials with Electrical resistivity of 7.3E-7 Ω·m

Chemical properties

PropertyValue

Carbon

0.06 %

Show Material materials with Carbon of 0.06 %

Chromium

18 - 20 %

Show Material materials with Chromium of 18 - 20 %

Manganese

2 %

Show Material materials with Manganese of 2 %

Nickel

8 - 11 %

Show Material materials with Nickel of 8 - 11 %

Nitrogen

0.12 - 0.22 %

Show Material materials with Nitrogen of 0.12 - 0.22 %

Phosphorus

0.05 %

Show Material materials with Phosphorus of 0.05 %

Silicon

1 %

Show Material materials with Silicon of 1 %

Sulfur

0.015 %

Show Material materials with Sulfur of 0.015 %