General
Property | Value | Temperature | Comment |
---|---|---|---|
Density | 7.9 - 8.2 g/cm³ Show Material materials with Density of 7.9 - 8.2 g/cm³ at 23.0 °C | 23.0 °C | Typical for Austenitic Stainless Steel |
Mechanical
Property | Value | Temperature | Comment |
---|---|---|---|
Elastic modulus | 195 GPa Show Material materials with Elastic modulus of 195 GPa at 23.0 °C | 23.0 °C | Typical for Austenitic Stainless Steel |
Elongation A50 | 9 % Show Material materials with Elongation A50 of 9 % at 23.0 °C | 23.0 °C | |
Poisson's ratio | 0.3 [-] Show Material materials with Poisson's ratio of 0.3 [-] at 23.0 °C | 23.0 °C | Typical for Austenitic Stainless Steel |
Shear modulus | 77 GPa Show Material materials with Shear modulus of 77 GPa at 23.0 °C | 23.0 °C | Typical for Austenitic Stainless Steel |
Tensile strength | 585 MPa Show Material materials with Tensile strength of 585 MPa at 23.0 °C | 23.0 °C | |
Yield strength | 275 MPa Show Material materials with Yield strength of 275 MPa at 23.0 °C | 23.0 °C |
Thermal
Property | Value | Temperature | Comment |
---|---|---|---|
Coefficient of thermal expansion | 1.7E-5 - 1.9E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.7E-5 - 1.9E-5 1/K at 23.0 °C | 23.0 °C | Typical for Austenitic Stainless Steel |
Melting point | 1230 - 1480 °C Show Material materials with Melting point of 1230 - 1480 °C | Typical for Austenitic Stainless Steel | |
Specific heat capacity | 440 J/(kg·K) Show Material materials with Specific heat capacity of 440 J/(kg·K) at 23.0 °C | 23.0 °C | Typical for Austenitic Stainless Steel |
Thermal conductivity | 11 - 21 W/(m·K) Show Material materials with Thermal conductivity of 11 - 21 W/(m·K) at 23.0 °C | 23.0 °C | Typical for Austenitic Stainless Steel |
Electrical
Property | Value | Temperature | Comment |
---|---|---|---|
Electrical resistivity | 8.5E-7 Ω·m Show Material materials with Electrical resistivity of 8.5E-7 Ω·m at 23.0 °C | 23.0 °C | Typical for Austenitic Stainless Steel |
Chemical properties
Property | ||
---|---|---|
Carbon | 0.2 - 0.5 % | |
Chromium | 26 - 30 % | |
Manganese | 2 % | |
Molybdenum | 0.5 % | |
Nickel | 8 - 11 % | |
Phosphorus | 0.04 % | |
Silicon | 2 % | |
Sulfur | 0.04 % |