General
Property | Value | Comment |
---|---|---|
Density | 7.8 - 7.9 g/cm³ Show Material materials with Density of 7.8 - 7.9 g/cm³ | Typical for Chromium Molybdenum Steel |
Mechanical
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Elastic modulus | 200 - 215 GPa Show Material materials with Elastic modulus of 200 - 215 GPa | Typical for Chromium Molybdenum Steel | |||
Elongation | 11.9 % Show Material materials with Elongation of 11.9 % | Predicted Value, A200 | |||
14 % Show Material materials with Elongation of 14 % | Quenched and Tempered | ASTM A542 | Plate | A50 | |
16.3 % Show Material materials with Elongation of 16.3 % | Predicted Value, A80 | ||||
18.1 % Show Material materials with Elongation of 18.1 % | Predicted Value, Transverse | ||||
19.8 % Show Material materials with Elongation of 19.8 % | Predicted Value | ||||
20.2 % Show Material materials with Elongation of 20.2 % | Predicted Value, A80 Transverse | ||||
Poisson's ratio | 0.29 [-] Show Material materials with Poisson's ratio of 0.29 [-] | Typical for Chromium Molybdenum Steel | |||
Reduction of area | 43.0 % Show Material materials with Reduction of area of 43.0 % | Predicted Value | |||
45.0 % Show Material materials with Reduction of area of 45.0 % | Predicted Value, Transverse | ||||
Shear modulus | 79.7 GPa Show Material materials with Shear modulus of 79.7 GPa | Predicted Value | |||
Shear strength | 674.3 MPa Show Material materials with Shear strength of 674.3 MPa | Predicted Value | |||
Tensile strength | 725 - 860 MPa Show Material materials with Tensile strength of 725 - 860 MPa | Quenched and Tempered | ASTM A542 | Plate | |
Yield strength | 301.2 MPa Show Material materials with Yield strength of 301.2 MPa | Predicted Value, RP1 | |||
329.7 MPa Show Material materials with Yield strength of 329.7 MPa | Predicted Value, RP1 Transverse | ||||
364.2 MPa Show Material materials with Yield strength of 364.2 MPa | Predicted Value, RP05 | ||||
496.6 MPa Show Material materials with Yield strength of 496.6 MPa | Predicted Value, Transverse | ||||
500.9 MPa Show Material materials with Yield strength of 500.9 MPa | Predicted Value, RP02 Transverse | ||||
585 MPa Show Material materials with Yield strength of 585 MPa | Quenched and Tempered | ASTM A542 | Plate | ||
602.3 MPa Show Material materials with Yield strength of 602.3 MPa | Predicted Value, RP02 | ||||
660.5 MPa Show Material materials with Yield strength of 660.5 MPa | Predicted Value, RP002 |
Thermal
Property | Value | Comment |
---|---|---|
Coefficient of thermal expansion | 1.1e-05 - 1.4e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.1e-05 - 1.4e-05 1/K | Typical for Chromium Molybdenum Steel |
Melting point | 1382 - 1529 °C Show Material materials with Melting point of 1382 - 1529 °C | Typical for Chromium Molybdenum Steel |
Specific heat capacity | 448 - 502 J/(kg·K) Show Material materials with Specific heat capacity of 448 - 502 J/(kg·K) | Typical for Chromium Molybdenum Steel |
Thermal conductivity | 36 - 43 W/(m·K) Show Material materials with Thermal conductivity of 36 - 43 W/(m·K) | Typical for Chromium Molybdenum Steel |
Electrical
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Carbon | 0.11 - 0.15 % Show Material materials with Carbon of 0.11 - 0.15 % | Quenched and Tempered | ASTM A542 | Plate |
Chromium | 2 - 2.5 % Show Material materials with Chromium of 2 - 2.5 % | Quenched and Tempered | ASTM A542 | Plate |
Copper | 0.25 % Show Material materials with Copper of 0.25 % | Quenched and Tempered | ASTM A542 | Plate |
Manganese | 0.3 - 0.6 % Show Material materials with Manganese of 0.3 - 0.6 % | Quenched and Tempered | ASTM A542 | Plate |
Molybdenum | 0.9 - 1.1 % Show Material materials with Molybdenum of 0.9 - 1.1 % | Quenched and Tempered | ASTM A542 | Plate |
Nickel | 0.25 % Show Material materials with Nickel of 0.25 % | Quenched and Tempered | ASTM A542 | Plate |
Phosphorus | 0.015 % Show Material materials with Phosphorus of 0.015 % | Quenched and Tempered | ASTM A542 | Plate |
Silicon | 0.5 % Show Material materials with Silicon of 0.5 % | Quenched and Tempered | ASTM A542 | Plate |
Sulfur | 0.015 % Show Material materials with Sulfur of 0.015 % | Quenched and Tempered | ASTM A542 | Plate |
Vanadium | 0.02 % Show Material materials with Vanadium of 0.02 % | Quenched and Tempered | ASTM A542 | Plate |
Technological properties
Property | ||
---|---|---|
Supplier Disclaimer | The given information is a rough description and some properties can depend on various factors such as product thickness. Please contact the supplier or refer to the related norm or standard for further information. |