Mechanical
Property | Temperature | Value |
---|---|---|
Charpy impact energy | 20.0 °C | 15 - 25 J Show Material materials with Charpy impact energy of 15 - 25 J |
Elongation | 20.0 °C | 9 - 13 % Show Material materials with Elongation of 9 - 13 % |
Reduction of area | 20.0 °C | 28 - 40 % Show Material materials with Reduction of area of 28 - 40 % |
Tensile strength | 20.0 °C | 1035 - 1450 MPa Show Material materials with Tensile strength of 1035 - 1450 MPa |
Yield Strength Rp0.2, short transverse | 20.0 °C | 965 - 1380 MPa Show Material materials with Yield Strength Rp0.2, short transverse of 965 - 1380 MPa |
Chemical properties
Property | Value |
---|---|
Carbon | 0.27 - 0.33 % Show Material materials with Carbon of 0.27 - 0.33 % |
Chromium | 0.8 - 1.1 % Show Material materials with Chromium of 0.8 - 1.1 % |
Manganese | 0.4 - 0.6 % Show Material materials with Manganese of 0.4 - 0.6 % |
Molybdenum | 0.15 - 0.25 % Show Material materials with Molybdenum of 0.15 - 0.25 % |
Phosphorus | 0.03 % Show Material materials with Phosphorus of 0.03 % |
Silicon | 0.2 - 0.35 % Show Material materials with Silicon of 0.2 - 0.35 % |
Sulfur | 0.025 % Show Material materials with Sulfur of 0.025 % |
Vanadium | 0.05 - 0.1 % Show Material materials with Vanadium of 0.05 - 0.1 % |