Description

The make X6Cr17 is comparable to X 6 Cr 17 acc. to DIN 17440 : 1985-07. The material is a ferritic steel (17% Cr). Largely resistant in water, steam, low acids and bases and in oxidizing acids (e.g. nitrous acid). As cold rolled sheet for washing machines and kitchen parts, canteens, facings, trim strips, bumper, wheel caps, in food and nitrous acid industry. Favorable deep draw and polishability for unwelded parts. In construction trade for decorative construction parts, e.g. for racks and furniture frames, safe deposit boxes, signs. A metallic clean surface is basic requirement for favorable corrosion resistance. X6Cr17 is applicated cold rolled resp. ground or polished. Resistance to intercrystalline corrosion in delivery condition but not in welded condition.

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

7.65 - 7.7 g/cm³

Show Material materials with Density of 7.65 - 7.7 g/cm³

Mechanical

PropertyTemperatureValue

Elastic modulus

20.0 °C

196 - 231.66 GPa

Show Material materials with Elastic modulus of 196 - 231.66 GPa

95.0 °C

227.53 GPa

Show Material materials with Elastic modulus of 227.53 GPa

100.0 °C

215 GPa

Show Material materials with Elastic modulus of 215 GPa

150.0 °C

223.39 GPa

Show Material materials with Elastic modulus of 223.39 GPa

200.0 °C

210 GPa

Show Material materials with Elastic modulus of 210 GPa

205.0 °C

218.56 GPa

Show Material materials with Elastic modulus of 218.56 GPa

260.0 °C

213.74 GPa

Show Material materials with Elastic modulus of 213.74 GPa

300.0 °C

205 GPa

Show Material materials with Elastic modulus of 205 GPa

315.0 °C

209.6 GPa

Show Material materials with Elastic modulus of 209.6 GPa

370.0 °C

204.09 GPa

Show Material materials with Elastic modulus of 204.09 GPa

400.0 °C

195 GPa

Show Material materials with Elastic modulus of 195 GPa

425.0 °C

198.57 GPa

Show Material materials with Elastic modulus of 198.57 GPa

485.0 °C

193.05 GPa

Show Material materials with Elastic modulus of 193.05 GPa

540.0 °C

187.54 GPa

Show Material materials with Elastic modulus of 187.54 GPa

595.0 °C

180.64 GPa

Show Material materials with Elastic modulus of 180.64 GPa

650.0 °C

173.06 GPa

Show Material materials with Elastic modulus of 173.06 GPa

705.0 °C

162.72 GPa

Show Material materials with Elastic modulus of 162.72 GPa

760.0 °C

151.69 GPa

Show Material materials with Elastic modulus of 151.69 GPa

815.0 °C

144.79 GPa

Show Material materials with Elastic modulus of 144.79 GPa

Hardness, Brinell

20.0 °C

200 [-]

Show Material materials with Hardness, Brinell of 200 [-]

Poisson's ratio

20.0 °C

0.24 [-]

Show Material materials with Poisson's ratio of 0.24 [-]

95.0 °C

0.27 [-]

Show Material materials with Poisson's ratio of 0.27 [-]

150.0 °C

0.28 [-]

Show Material materials with Poisson's ratio of 0.28 [-]

205.0 °C

0.29 [-]

Show Material materials with Poisson's ratio of 0.29 [-]

260.0 °C

0.29 [-]

Show Material materials with Poisson's ratio of 0.29 [-]

315.0 °C

0.29 [-]

Show Material materials with Poisson's ratio of 0.29 [-]

370.0 °C

0.29 [-]

Show Material materials with Poisson's ratio of 0.29 [-]

425.0 °C

0.29 [-]

Show Material materials with Poisson's ratio of 0.29 [-]

485.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

540.0 °C

0.31 [-]

Show Material materials with Poisson's ratio of 0.31 [-]

595.0 °C

0.31 [-]

Show Material materials with Poisson's ratio of 0.31 [-]

650.0 °C

0.34 [-]

Show Material materials with Poisson's ratio of 0.34 [-]

705.0 °C

0.34 [-]

Show Material materials with Poisson's ratio of 0.34 [-]

760.0 °C

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

815.0 °C

0.35 [-]

Show Material materials with Poisson's ratio of 0.35 [-]

Unlock all property charts

Shear modulus

20.0 °C

93.08 GPa

Show Material materials with Shear modulus of 93.08 GPa

95.0 °C

89.63 GPa

Show Material materials with Shear modulus of 89.63 GPa

150.0 °C

87.56 GPa

Show Material materials with Shear modulus of 87.56 GPa

205.0 °C

84.81 GPa

Show Material materials with Shear modulus of 84.81 GPa

260.0 °C

82.74 GPa

Show Material materials with Shear modulus of 82.74 GPa

315.0 °C

81.36 GPa

Show Material materials with Shear modulus of 81.36 GPa

370.0 °C

79.29 GPa

Show Material materials with Shear modulus of 79.29 GPa

425.0 °C

77.22 GPa

Show Material materials with Shear modulus of 77.22 GPa

485.0 °C

74.46 GPa

Show Material materials with Shear modulus of 74.46 GPa

540.0 °C

71.71 GPa

Show Material materials with Shear modulus of 71.71 GPa

595.0 °C

68.95 GPa

Show Material materials with Shear modulus of 68.95 GPa

650.0 °C

64.81 GPa

Show Material materials with Shear modulus of 64.81 GPa

705.0 °C

60.67 GPa

Show Material materials with Shear modulus of 60.67 GPa

760.0 °C

57.23 GPa

Show Material materials with Shear modulus of 57.23 GPa

815.0 °C

53.78 GPa

Show Material materials with Shear modulus of 53.78 GPa

Unlock all property charts

Tensile strength

20.0 °C

400 - 630 MPa

Show Material materials with Tensile strength of 400 - 630 MPa

Yield strength Rp0.2

20.0 °C

240 MPa

Show Material materials with Yield strength Rp0.2 of 240 MPa

100.0 °C

220 MPa

Show Material materials with Yield strength Rp0.2 of 220 MPa

150.0 °C

215 MPa

Show Material materials with Yield strength Rp0.2 of 215 MPa

200.0 °C

210 MPa

Show Material materials with Yield strength Rp0.2 of 210 MPa

250.0 °C

205 MPa

Show Material materials with Yield strength Rp0.2 of 205 MPa

300.0 °C

200 MPa

Show Material materials with Yield strength Rp0.2 of 200 MPa

350.0 °C

195 MPa

Show Material materials with Yield strength Rp0.2 of 195 MPa

400.0 °C

190 MPa

Show Material materials with Yield strength Rp0.2 of 190 MPa

Unlock all property charts

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

-100.0 °C

9.2E-6 1/K

Show Material materials with Coefficient of thermal expansion of 9.2E-6 1/K

20.0 °C

9.9E-6 1/K

Show Material materials with Coefficient of thermal expansion of 9.9E-6 1/K

100.0 °C

1E-5 - 1.03E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1E-5 - 1.03E-5 1/K

200.0 °C

1E-5 - 1.08E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1E-5 - 1.08E-5 1/K

300.0 °C

1.05E-5 - 1.12E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.05E-5 - 1.12E-5 1/K

400.0 °C

1.05E-5 - 1.16E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.05E-5 - 1.16E-5 1/K

500.0 °C

1.1E-5 - 1.19E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.1E-5 - 1.19E-5 1/K

600.0 °C

1.21E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.21E-5 1/K

700.0 °C

1.24E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.24E-5 1/K

800.0 °C

1.29E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.29E-5 1/K

900.0 °C

1.34E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.34E-5 1/K

1000.0 °C

1.39E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.39E-5 1/K

Unlock all property charts

Melting point

1425 - 1530 °C

Show Material materials with Melting point of 1425 - 1530 °C

Typical for Ferritic Stainless Steel

Specific heat capacity

20.0 °C

450 - 460 J/(kg·K)

Show Material materials with Specific heat capacity of 450 - 460 J/(kg·K)

100.0 °C

482 J/(kg·K)

Show Material materials with Specific heat capacity of 482 J/(kg·K)

200.0 °C

506 J/(kg·K)

Show Material materials with Specific heat capacity of 506 J/(kg·K)

300.0 °C

525 J/(kg·K)

Show Material materials with Specific heat capacity of 525 J/(kg·K)

400.0 °C

547 J/(kg·K)

Show Material materials with Specific heat capacity of 547 J/(kg·K)

500.0 °C

576 J/(kg·K)

Show Material materials with Specific heat capacity of 576 J/(kg·K)

600.0 °C

616 J/(kg·K)

Show Material materials with Specific heat capacity of 616 J/(kg·K)

Unlock all property charts

Thermal conductivity

20.0 °C

19.6 - 25 W/(m·K)

Show Material materials with Thermal conductivity of 19.6 - 25 W/(m·K)

Thermal diffusivity

20.0 °C

5.7 mm²/s

Show Material materials with Thermal diffusivity of 5.7 mm²/s

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

6.17E-7 Ω·m

Show Material materials with Electrical resistivity of 6.17E-7 Ω·m

Chemical properties

PropertyValue

Carbon

0.08 %

Show Material materials with Carbon of 0.08 %

Chromium

16 - 18 %

Show Material materials with Chromium of 16 - 18 %

Manganese

1 %

Show Material materials with Manganese of 1 %

Phosphorus

0.04 %

Show Material materials with Phosphorus of 0.04 %

Silicon

1 %

Show Material materials with Silicon of 1 %

Sulfur

0.03 %

Show Material materials with Sulfur of 0.03 %