General
Property | Temperature | Value | Comment |
---|---|---|---|
Density | 23.0 °C | 7.6 - 7.7 g/cm³ Show Material materials with Density of 7.6 - 7.7 g/cm³ | Typical for Martensitic Stainless Steel |
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Charpy impact energy | 23.0 °C | 11 J Show Material materials with Charpy impact energy of 11 J | |
Elastic modulus | 23.0 °C | 220 GPa Show Material materials with Elastic modulus of 220 GPa | Typical for Martensitic Stainless Steel |
Elongation A50 | 23.0 °C | 13 % Show Material materials with Elongation A50 of 13 % | |
Hardness, Brinell | 23.0 °C | 302 - 352 [-] Show Material materials with Hardness, Brinell of 302 - 352 [-] | |
Poisson's ratio | 23.0 °C | 0.3 [-] Show Material materials with Poisson's ratio of 0.3 [-] | Typical for Martensitic Stainless Steel |
Reduction of area | 23.0 °C | 30 % Show Material materials with Reduction of area of 30 % | |
Shear modulus | 23.0 °C | 77 GPa Show Material materials with Shear modulus of 77 GPa | Typical for Martensitic Stainless Steel |
Tensile strength | 23.0 °C | 965 MPa Show Material materials with Tensile strength of 965 MPa | |
Yield strength Rp0.2 | 23.0 °C | 760 MPa Show Material materials with Yield strength Rp0.2 of 760 MPa |
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of thermal expansion | 23.0 °C | 1E-5 - 1.5E-5 1/K Show Material materials with Coefficient of thermal expansion of 1E-5 - 1.5E-5 1/K | Typical for Martensitic Stainless Steel |
Melting point | 1370 - 1530 °C Show Material materials with Melting point of 1370 - 1530 °C | Typical for Martensitic Stainless Steel | |
Specific heat capacity | 23.0 °C | 460 J/(kg·K) Show Material materials with Specific heat capacity of 460 J/(kg·K) | Typical for Martensitic Stainless Steel |
Thermal conductivity | 23.0 °C | 14 - 31 W/(m·K) Show Material materials with Thermal conductivity of 14 - 31 W/(m·K) | Typical for Martensitic Stainless Steel |
Electrical
Property | Temperature | Value | Comment |
---|---|---|---|
Electrical resistivity | 23.0 °C | 6E-7 Ω·m Show Material materials with Electrical resistivity of 6E-7 Ω·m | Typical for Martensitic Stainless Steel |
Chemical properties
Property | Value |
---|---|
Carbon | 0.2 - 0.25 % Show Material materials with Carbon of 0.2 - 0.25 % |
Chromium | 11 - 12.5 % Show Material materials with Chromium of 11 - 12.5 % |
Manganese | 0.5 - 1 % Show Material materials with Manganese of 0.5 - 1 % |
Molybdenum | 0.9 - 1.25 % Show Material materials with Molybdenum of 0.9 - 1.25 % |
Nickel | 0.5 - 1 % Show Material materials with Nickel of 0.5 - 1 % |
Phosphorus | 0.03 % Show Material materials with Phosphorus of 0.03 % |
Silicon | 0.5 % Show Material materials with Silicon of 0.5 % |
Sulfur | 0.025 % Show Material materials with Sulfur of 0.025 % |
Tungsten | 0.9 - 1.25 % Show Material materials with Tungsten of 0.9 - 1.25 % |
Vanadium | 0.2 - 0.3 % Show Material materials with Vanadium of 0.2 - 0.3 % |