ASTM A350 Grade LF3 Class 1 Heat-Treated

Want to keep this datasheet? Save it now in your required format

Related Standards

Equivalent Materials

This material data has been provided by ASTM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueComment

Density

23.0 °C

8.8 g/cm³

Show Material materials with Density of 8.8 g/cm³

Typical for Nickel Steel

Mechanical

PropertyTemperatureValueComment

Charpy impact energy

23.0 °C

20 J

Show Material materials with Charpy impact energy of 20 J

Elastic modulus

23.0 °C

200 - 215 GPa

Show Material materials with Elastic modulus of 200 - 215 GPa

Typical for Nickel Steel

Elongation A50

23.0 °C

30 %

Show Material materials with Elongation A50 of 30 %

Poisson's ratio

23.0 °C

0.29 [-]

Show Material materials with Poisson's ratio of 0.29 [-]

Typical for Nickel Steel

Reduction of area

23.0 °C

35 %

Show Material materials with Reduction of area of 35 %

Shear modulus

23.0 °C

76 GPa

Show Material materials with Shear modulus of 76 GPa

Typical for Nickel Steel

Tensile strength

23.0 °C

485 - 655 MPa

Show Material materials with Tensile strength of 485 - 655 MPa

Yield strength Rp0.2

23.0 °C

260 MPa

Show Material materials with Yield strength Rp0.2 of 260 MPa

Thermal

PropertyTemperatureValueComment

Melting point

1316 - 1595 °C

Show Material materials with Melting point of 1316 - 1595 °C

Typical for Nickel Steel

Specific heat capacity

23.0 °C

456 J/(kg·K)

Show Material materials with Specific heat capacity of 456 J/(kg·K)

Typical for Nickel Steel

Thermal conductivity

23.0 °C

10 - 50 W/(m·K)

Show Material materials with Thermal conductivity of 10 - 50 W/(m·K)

Typical for Nickel Steel

Chemical properties

PropertyValue

Carbon

0.2 %

Show Material materials with Carbon of 0.2 %

Chromium

0.3 %

Show Material materials with Chromium of 0.3 %

Copper

0.4 %

Show Material materials with Copper of 0.4 %

Manganese

0.9 %

Show Material materials with Manganese of 0.9 %

Molybdenum

0.12 %

Show Material materials with Molybdenum of 0.12 %

Nickel

3.3 - 3.7 %

Show Material materials with Nickel of 3.3 - 3.7 %

Niobium

0.02 %

Show Material materials with Niobium of 0.02 %

Phosphorus

0.04 %

Show Material materials with Phosphorus of 0.04 %

Silicon

0.2 - 0.35 %

Show Material materials with Silicon of 0.2 - 0.35 %

Sulfur

0.04 %

Show Material materials with Sulfur of 0.04 %

Vanadium

0.03 %

Show Material materials with Vanadium of 0.03 %