EN 10025-2 Grade S235J2 normalized or normalized formed (+N)

View suppliers (32)
Want to keep this datasheet? Save it now in your required format

Description

The hot rolled, unalloyed quality steel S235J2 is a fine grained steel for welding constructions for alternate loading. The steel is not intended for heat treatment. Stress relieving annealing is allowed. Products in the delivery condition +N may be hot formed and/or normalized after delivery. For long products and continuous rolled flats the delivery condition is up to the producer +AR, +N or +M. The delivery condition of four-high rolled sheet is also up to the producer and may be +AR or +N. Both conditions can be ordered. For this steel are available (mat. no 1.0119, S235J2C) grades for folding, roll forming to shape and cold drawing. The steel grade S235J2 (1.0117) replaces the steel grade S235J2G3 (1.0116) according to EN 10025 (1994-03).

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

"Typical" values were obtained via a literature search. "Predicted" values were imputed via artificial intelligence technology. While we have placed significant efforts in ensuring data accuracy, "typical" and "predicted" data should be considered indicative and verified by appropriate material testing. Please do contact us if additional information on the the predicted data method is required.
All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValueComment

Density

7.8 - 7.9 g/cm³

Show Material materials with Density of 7.8 - 7.9 g/cm³

Typical for Low Carbon Steel

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Elastic modulus

200 - 215 GPa

Show Material materials with Elastic modulus of 200 - 215 GPa

Typical for Low Carbon Steel

Elongation

18.4 %

Show Material materials with Elongation of 18.4 %

Predicted Value, A200

21.4 %

Show Material materials with Elongation of 21.4 %

Predicted Value, A5

26.6 %

Show Material materials with Elongation of 26.6 %

Predicted Value, A50

20 °C

15 %

Show Material materials with Elongation of 15 %

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

A80 Transverse

20 °C

16 %

Show Material materials with Elongation of 16 %

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

A80 Transverse

20 °C

17 %

Show Material materials with Elongation of 17 %

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

A80 Transverse

20 °C

17 %

Show Material materials with Elongation of 17 %

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

A80

20 °C

18 %

Show Material materials with Elongation of 18 %

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

A80 Transverse

20 °C

18 %

Show Material materials with Elongation of 18 %

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

A80

20 °C

19 %

Show Material materials with Elongation of 19 %

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

A80 Transverse

20 °C

19 %

Show Material materials with Elongation of 19 %

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

A80

20 °C

20 %

Show Material materials with Elongation of 20 %

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

A80

20 °C

21 %

Show Material materials with Elongation of 21 %

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

A80

20 °C

21 %

Show Material materials with Elongation of 21 %

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

Transverse

20 °C

21 %

Show Material materials with Elongation of 21 %

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

20 °C

22 %

Show Material materials with Elongation of 22 %

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

Transverse

20 °C

22 %

Show Material materials with Elongation of 22 %

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

20 °C

23 %

Show Material materials with Elongation of 23 %

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

Transverse

20 °C

24 %

Show Material materials with Elongation of 24 %

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

Transverse

20 °C

24 %

Show Material materials with Elongation of 24 %

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

20 °C

26 %

Show Material materials with Elongation of 26 %

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

Hardness, Brinell

249 [-]

Show Material materials with Hardness, Brinell of 249 [-]

Predicted Value, Transverse

Poisson's ratio

20 °C

0.284 [-]

Show Material materials with Poisson's ratio of 0.284 [-]

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

Reduction of area

44.1 %

Show Material materials with Reduction of area of 44.1 %

Predicted Value, Transverse

50.8 %

Show Material materials with Reduction of area of 50.8 %

Predicted Value

Shear modulus

82 GPa

Show Material materials with Shear modulus of 82 GPa

Typical for Low Carbon Steel

Shear strength

511.9 MPa

Show Material materials with Shear strength of 511.9 MPa

Predicted Value

Tensile strength

20 °C

330 - 510 MPa

Show Material materials with Tensile strength of 330 - 510 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

20 °C

330 - 500 MPa

Show Material materials with Tensile strength of 330 - 500 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

20 °C

330 - 490 MPa

Show Material materials with Tensile strength of 330 - 490 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

20 °C

330 - 480 MPa

Show Material materials with Tensile strength of 330 - 480 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

20 °C

340 - 510 MPa

Show Material materials with Tensile strength of 340 - 510 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

20 °C

340 - 500 MPa

Show Material materials with Tensile strength of 340 - 500 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

20 °C

340 - 490 MPa

Show Material materials with Tensile strength of 340 - 490 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

20 °C

340 - 480 MPa

Show Material materials with Tensile strength of 340 - 480 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

20 °C

350 - 510 MPa

Show Material materials with Tensile strength of 350 - 510 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

20 °C

350 - 500 MPa

Show Material materials with Tensile strength of 350 - 500 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

20 °C

350 - 490 MPa

Show Material materials with Tensile strength of 350 - 490 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

20 °C

350 - 480 MPa

Show Material materials with Tensile strength of 350 - 480 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

20 °C

360 - 510 MPa

Show Material materials with Tensile strength of 360 - 510 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

20 °C

360 - 500 MPa

Show Material materials with Tensile strength of 360 - 500 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

20 °C

360 - 490 MPa

Show Material materials with Tensile strength of 360 - 490 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

20 °C

360 - 480 MPa

Show Material materials with Tensile strength of 360 - 480 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

Yield strength

263.7 MPa

Show Material materials with Yield strength of 263.7 MPa

Predicted Value, RP1

269.2 MPa

Show Material materials with Yield strength of 269.2 MPa

Predicted Value, RP05

278.1 MPa

Show Material materials with Yield strength of 278.1 MPa

Predicted Value, Transverse

320.4 MPa

Show Material materials with Yield strength of 320.4 MPa

Predicted Value, RP1 Transverse

349.1 MPa

Show Material materials with Yield strength of 349.1 MPa

Predicted Value, RP02

445.3 MPa

Show Material materials with Yield strength of 445.3 MPa

Predicted Value, RP02 Transverse

468.1 MPa

Show Material materials with Yield strength of 468.1 MPa

Predicted Value, RP002

20 °C

165 MPa

Show Material materials with Yield strength of 165 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

20 °C

175 MPa

Show Material materials with Yield strength of 175 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

20 °C

185 MPa

Show Material materials with Yield strength of 185 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

20 °C

195 MPa

Show Material materials with Yield strength of 195 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

20 °C

215 MPa

Show Material materials with Yield strength of 215 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

20 °C

225 MPa

Show Material materials with Yield strength of 225 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

20 °C

235 MPa

Show Material materials with Yield strength of 235 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

100 °C

159 - 187 MPa

Show Material materials with Yield strength of 159 - 187 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

100 °C

159 - 180 MPa

Show Material materials with Yield strength of 159 - 180 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

100 °C

159 - 173 MPa

Show Material materials with Yield strength of 159 - 173 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

100 °C

159 MPa

Show Material materials with Yield strength of 159 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

100 °C

173 - 187 MPa

Show Material materials with Yield strength of 173 - 187 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

100 °C

173 - 180 MPa

Show Material materials with Yield strength of 173 - 180 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

100 °C

173 MPa

Show Material materials with Yield strength of 173 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

100 °C

180 - 187 MPa

Show Material materials with Yield strength of 180 - 187 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

100 °C

180 MPa

Show Material materials with Yield strength of 180 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

100 °C

187 MPa

Show Material materials with Yield strength of 187 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

200 °C

137 - 161 MPa

Show Material materials with Yield strength of 137 - 161 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

200 °C

137 - 155 MPa

Show Material materials with Yield strength of 137 - 155 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

200 °C

137 - 149 MPa

Show Material materials with Yield strength of 137 - 149 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

200 °C

137 MPa

Show Material materials with Yield strength of 137 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

200 °C

149 - 161 MPa

Show Material materials with Yield strength of 149 - 161 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

200 °C

149 - 155 MPa

Show Material materials with Yield strength of 149 - 155 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

200 °C

149 MPa

Show Material materials with Yield strength of 149 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

200 °C

155 - 161 MPa

Show Material materials with Yield strength of 155 - 161 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

200 °C

155 MPa

Show Material materials with Yield strength of 155 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

200 °C

161 MPa

Show Material materials with Yield strength of 161 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

250 °C

115 - 143 MPa

Show Material materials with Yield strength of 115 - 143 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

250 °C

115 - 136 MPa

Show Material materials with Yield strength of 115 - 136 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

250 °C

115 - 129 MPa

Show Material materials with Yield strength of 115 - 129 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

250 °C

115 MPa

Show Material materials with Yield strength of 115 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

250 °C

129 - 143 MPa

Show Material materials with Yield strength of 129 - 143 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

250 °C

129 - 136 MPa

Show Material materials with Yield strength of 129 - 136 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

250 °C

129 MPa

Show Material materials with Yield strength of 129 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

250 °C

136 - 143 MPa

Show Material materials with Yield strength of 136 - 143 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

250 °C

136 MPa

Show Material materials with Yield strength of 136 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

250 °C

143 MPa

Show Material materials with Yield strength of 143 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

300 °C

102 - 122 MPa

Show Material materials with Yield strength of 102 - 122 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

300 °C

102 - 117 MPa

Show Material materials with Yield strength of 102 - 117 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

300 °C

102 - 112 MPa

Show Material materials with Yield strength of 102 - 112 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

300 °C

102 MPa

Show Material materials with Yield strength of 102 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

300 °C

112 - 122 MPa

Show Material materials with Yield strength of 112 - 122 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

300 °C

112 - 117 MPa

Show Material materials with Yield strength of 112 - 117 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

300 °C

112 MPa

Show Material materials with Yield strength of 112 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

300 °C

117 - 122 MPa

Show Material materials with Yield strength of 117 - 122 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

300 °C

117 MPa

Show Material materials with Yield strength of 117 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

300 °C

122 MPa

Show Material materials with Yield strength of 122 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Thermal

PropertyValueComment

Coefficient of thermal expansion

1.32e-05 - 1.38e-05 1/K

Show Material materials with Coefficient of thermal expansion of 1.32e-05 - 1.38e-05 1/K

Typical for Low Carbon Steel

Max service temperature

294.5 °C

Show Material materials with Max service temperature of 294.5 °C

Predicted Value, Long

500 °C

Show Material materials with Max service temperature of 500 °C

Typical for Carbon Steel

Melting point

1480 - 1526 °C

Show Material materials with Melting point of 1480 - 1526 °C

Typical for Low Carbon Steel

Specific heat capacity

465 J/(kg·K)

Show Material materials with Specific heat capacity of 465 J/(kg·K)

Typical for Low Carbon Steel

Thermal conductivity

25 - 93 W/(m·K)

Show Material materials with Thermal conductivity of 25 - 93 W/(m·K)

Typical for Low Carbon Steel

Electrical

PropertyValueComment

Electrical conductivity

7 S/m

Show Material materials with Electrical conductivity of 7 S/m

Predicted Value

Electrical resistivity

1.43e-07 - 1.74e-07 Ω·m

Show Material materials with Electrical resistivity of 1.43e-07 - 1.74e-07 Ω·m

Typical for Carbon Steel

Magnetic

PropertyValueComment

Curie temperature

770 °C

Show Material materials with Curie temperature of 770 °C

Typical for Low Carbon Steel

Chemical properties

PropertyValueConditionRelated StandardsShape

Carbon

0.17 %

Show Material materials with Carbon of 0.17 %

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

Copper

0.55 %

Show Material materials with Copper of 0.55 %

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

Manganese

1.4 %

Show Material materials with Manganese of 1.4 %

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

Phosphorus

0.025 %

Show Material materials with Phosphorus of 0.025 %

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

Sulfur

0.025 %

Show Material materials with Sulfur of 0.025 %

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

Technological properties

Property
Supplier Disclaimer

The given information is a rough description and some properties can depend on various factors such as product thickness. Please contact the supplier or refer to the related norm or standard for further information.

Do you have a technical question or need more information about this material?

Post it as a comment below and receive answers from engineers and other community members.