General
Property | Temperature | Value |
---|---|---|
Density | 23.0 °C | 7.8 g/cm³ Show Material materials with Density of 7.8 g/cm³ |
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elastic modulus | 23.0 °C | 210 GPa Show Material materials with Elastic modulus of 210 GPa | |
Elongation | 23.0 °C | 26 % Show Material materials with Elongation of 26 % | |
Poisson's ratio | 23.0 °C | 0.29 [-] Show Material materials with Poisson's ratio of 0.29 [-] | Typical for Chromium Molybdenum Steel |
Tensile strength | 23.0 °C | 640 MPa Show Material materials with Tensile strength of 640 MPa | |
Yield strength | 23.0 °C | 360 MPa Show Material materials with Yield strength of 360 MPa |
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of thermal expansion | 23.0 °C | 1.2E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.2E-5 1/K | |
Melting point | 1382 - 1529 °C Show Material materials with Melting point of 1382 - 1529 °C | Typical for Chromium Molybdenum Steel | |
Specific heat capacity | 23.0 °C | 450 J/(kg·K) Show Material materials with Specific heat capacity of 450 J/(kg·K) | |
Thermal conductivity | 23.0 °C | 36 - 43 W/(m·K) Show Material materials with Thermal conductivity of 36 - 43 W/(m·K) | Typical for Chromium Molybdenum Steel |
Chemical properties
Property | Value |
---|---|
Carbon | 0.18 - 0.23 % Show Material materials with Carbon of 0.18 - 0.23 % |
Chromium | 0.4 - 0.6 % Show Material materials with Chromium of 0.4 - 0.6 % |
Iron | 96.9 - 98 % Show Material materials with Iron of 96.9 - 98 % |
Manganese | 0.7 - 0.9 % Show Material materials with Manganese of 0.7 - 0.9 % |
Molybdenum | 0.15 - 0.25 % Show Material materials with Molybdenum of 0.15 - 0.25 % |
Nickel | 0.4 - 0.7 % Show Material materials with Nickel of 0.4 - 0.7 % |
Phosphorus | 0 - 0.04 % Show Material materials with Phosphorus of 0 - 0.04 % |
Silicon | 0.15 - 0.35 % Show Material materials with Silicon of 0.15 - 0.35 % |
Sulfur | 0 - 0.04 % Show Material materials with Sulfur of 0 - 0.04 % |