EN 10088-4 Grade X2CrTi12 soft annealed (+A)

Want to keep this datasheet? Save it now in your required format

Description

Properties are in DIN EN 10088-2 : 2005-09 / Material variant DIN EN 10088-1 :2005-09

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

7.7 - 7.73 g/cm³

Show Material materials with Density of 7.7 - 7.73 g/cm³

Mechanical

PropertyTemperatureValue

Elastic modulus

20.0 °C

217 - 220 GPa

Show Material materials with Elastic modulus of 217 - 220 GPa

100.0 °C

215 GPa

Show Material materials with Elastic modulus of 215 GPa

200.0 °C

188 - 210 GPa

Show Material materials with Elastic modulus of 188 - 210 GPa

300.0 °C

164 - 205 GPa

Show Material materials with Elastic modulus of 164 - 205 GPa

400.0 °C

195 GPa

Show Material materials with Elastic modulus of 195 GPa

Elongation

20.0 °C

25 %

Show Material materials with Elongation of 25 %

Elongation A80

20.0 °C

25 %

Show Material materials with Elongation A80 of 25 %

Elongation A80, transverse

20.0 °C

25 %

Show Material materials with Elongation A80, transverse of 25 %

Elongation, transverse

20.0 °C

25 %

Show Material materials with Elongation, transverse of 25 %

Poisson's ratio

20.0 °C

0.29 [-]

Show Material materials with Poisson's ratio of 0.29 [-]

Shear modulus

20.0 °C

84.82 GPa

Show Material materials with Shear modulus of 84.82 GPa

Tensile strength

20.0 °C

380 - 560 MPa

Show Material materials with Tensile strength of 380 - 560 MPa

Tensile strength, transverse

20.0 °C

380 - 560 MPa

Show Material materials with Tensile strength, transverse of 380 - 560 MPa

Yield strength Rp0.2

20.0 °C

210 MPa

Show Material materials with Yield strength Rp0.2 of 210 MPa

100.0 °C

200 MPa

Show Material materials with Yield strength Rp0.2 of 200 MPa

150.0 °C

195 MPa

Show Material materials with Yield strength Rp0.2 of 195 MPa

200.0 °C

190 MPa

Show Material materials with Yield strength Rp0.2 of 190 MPa

250.0 °C

186 MPa

Show Material materials with Yield strength Rp0.2 of 186 MPa

300.0 °C

180 MPa

Show Material materials with Yield strength Rp0.2 of 180 MPa

350.0 °C

160 MPa

Show Material materials with Yield strength Rp0.2 of 160 MPa

Unlock all property charts

Yield strength Rp0.2, transverse

20.0 °C

220 MPa

Show Material materials with Yield strength Rp0.2, transverse of 220 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

20.0 °C

1.02E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.02E-5 1/K

100.0 °C

1.05E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.05E-5 1/K

200.0 °C

1.09E-5 - 1.1E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.09E-5 - 1.1E-5 1/K

300.0 °C

1.13E-5 - 1.15E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.13E-5 - 1.15E-5 1/K

400.0 °C

1.16E-5 - 1.2E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.16E-5 - 1.2E-5 1/K

500.0 °C

1.2E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.2E-5 1/K

600.0 °C

1.22E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.22E-5 1/K

Unlock all property charts

Melting point

1425 - 1530 °C

Show Material materials with Melting point of 1425 - 1530 °C

Typical for Ferritic Stainless Steel

Specific heat capacity

20.0 °C

439 - 460 J/(kg·K)

Show Material materials with Specific heat capacity of 439 - 460 J/(kg·K)

100.0 °C

474 J/(kg·K)

Show Material materials with Specific heat capacity of 474 J/(kg·K)

200.0 °C

498 J/(kg·K)

Show Material materials with Specific heat capacity of 498 J/(kg·K)

300.0 °C

517 J/(kg·K)

Show Material materials with Specific heat capacity of 517 J/(kg·K)

400.0 °C

538 J/(kg·K)

Show Material materials with Specific heat capacity of 538 J/(kg·K)

500.0 °C

564 J/(kg·K)

Show Material materials with Specific heat capacity of 564 J/(kg·K)

600.0 °C

598 J/(kg·K)

Show Material materials with Specific heat capacity of 598 J/(kg·K)

Unlock all property charts

Thermal conductivity

20.0 °C

25 - 25.9 W/(m·K)

Show Material materials with Thermal conductivity of 25 - 25.9 W/(m·K)

100.0 °C

25.3 W/(m·K)

Show Material materials with Thermal conductivity of 25.3 W/(m·K)

200.0 °C

25.2 W/(m·K)

Show Material materials with Thermal conductivity of 25.2 W/(m·K)

300.0 °C

25.2 W/(m·K)

Show Material materials with Thermal conductivity of 25.2 W/(m·K)

400.0 °C

25.4 W/(m·K)

Show Material materials with Thermal conductivity of 25.4 W/(m·K)

500.0 °C

25.7 W/(m·K)

Show Material materials with Thermal conductivity of 25.7 W/(m·K)

600.0 °C

25.9 W/(m·K)

Show Material materials with Thermal conductivity of 25.9 W/(m·K)

Unlock all property charts

Thermal diffusivity

20.0 °C

7.6 mm²/s

Show Material materials with Thermal diffusivity of 7.6 mm²/s

100.0 °C

6.6 mm²/s

Show Material materials with Thermal diffusivity of 6.6 mm²/s

200.0 °C

6.1 mm²/s

Show Material materials with Thermal diffusivity of 6.1 mm²/s

300.0 °C

5.8 mm²/s

Show Material materials with Thermal diffusivity of 5.8 mm²/s

400.0 °C

5.3 mm²/s

Show Material materials with Thermal diffusivity of 5.3 mm²/s

500.0 °C

4.8 mm²/s

Show Material materials with Thermal diffusivity of 4.8 mm²/s

600.0 °C

4.1 mm²/s

Show Material materials with Thermal diffusivity of 4.1 mm²/s

Unlock all property charts

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

5.59E-7 - 6E-7 Ω·m

Show Material materials with Electrical resistivity of 5.59E-7 - 6E-7 Ω·m

100.0 °C

6.4E-7 Ω·m

Show Material materials with Electrical resistivity of 6.4E-7 Ω·m

200.0 °C

7.32E-7 Ω·m

Show Material materials with Electrical resistivity of 7.32E-7 Ω·m

300.0 °C

8.17E-7 Ω·m

Show Material materials with Electrical resistivity of 8.17E-7 Ω·m

400.0 °C

8.97E-7 Ω·m

Show Material materials with Electrical resistivity of 8.97E-7 Ω·m

500.0 °C

9.74E-7 Ω·m

Show Material materials with Electrical resistivity of 9.74E-7 Ω·m

600.0 °C

1.05E-6 Ω·m

Show Material materials with Electrical resistivity of 1.05E-6 Ω·m

Unlock all property charts

Chemical properties

PropertyValue

Carbon

0.03 %

Show Material materials with Carbon of 0.03 %

Chromium

10.5 - 12.5 %

Show Material materials with Chromium of 10.5 - 12.5 %

Manganese

1 %

Show Material materials with Manganese of 1 %

Phosphorus

0.04 %

Show Material materials with Phosphorus of 0.04 %

Silicon

1 %

Show Material materials with Silicon of 1 %

Sulfur

0.015 %

Show Material materials with Sulfur of 0.015 %

Titanium

0.65 %

Show Material materials with Titanium of 0.65 %