Material X50CrMoV15 is comparable to X 45 CrMoV 15 acc. to DIN 17440:1985-07. Hardenable steel of high strength and high abrasion resistance for all kinds of cutting tools, especially for partial hardened cutting tools, for ball bearing balls, wear resistant components, controlling and pump parts. Resistant to water and steam in hardened condition. Higher resistance than 1.4034 and 1.4110. Insufficient corrosion resistance in annealed or high tempered condition.

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

7.56 - 7.7 g/cm³

Show Material materials with Density of 7.56 - 7.7 g/cm³

Mechanical

PropertyTemperatureValueComment

Elastic modulus

20.0 °C

215 - 218 GPa

Show Material materials with Elastic modulus of 215 - 218 GPa

100.0 °C

212 - 213 GPa

Show Material materials with Elastic modulus of 212 - 213 GPa

200.0 °C

205 - 206 GPa

Show Material materials with Elastic modulus of 205 - 206 GPa

300.0 °C

198 - 200 GPa

Show Material materials with Elastic modulus of 198 - 200 GPa

400.0 °C

190 GPa

Show Material materials with Elastic modulus of 190 GPa

500.0 °C

180 GPa

Show Material materials with Elastic modulus of 180 GPa

600.0 °C

167 GPa

Show Material materials with Elastic modulus of 167 GPa

700.0 °C

150 GPa

Show Material materials with Elastic modulus of 150 GPa

Elongation

20.0 °C

12 %

Show Material materials with Elongation of 12 %

Elongation A80

20.0 °C

12 %

Show Material materials with Elongation A80 of 12 %

Hardness, Brinell

20.0 °C

280 [-]

Show Material materials with Hardness, Brinell of 280 [-]

Hardness, Rockwell B

20.0 °C

100 [-]

Show Material materials with Hardness, Rockwell B of 100 [-]

Hardness, Vickers

20.0 °C

280 [-]

Show Material materials with Hardness, Vickers of 280 [-]

Poisson's ratio

23.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

Typical for Martensitic Stainless Steel

Shear modulus

23.0 °C

77 GPa

Show Material materials with Shear modulus of 77 GPa

Typical for Martensitic Stainless Steel

Tensile strength

20.0 °C

850 - 900 MPa

Show Material materials with Tensile strength of 850 - 900 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

20.0 °C

9.9E-6 1/K

Show Material materials with Coefficient of thermal expansion of 9.9E-6 1/K

100.0 °C

1.03E-5 - 1.05E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.03E-5 - 1.05E-5 1/K

200.0 °C

1.08E-5 - 1.1E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.08E-5 - 1.1E-5 1/K

300.0 °C

1.1E-5 - 1.12E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.1E-5 - 1.12E-5 1/K

400.0 °C

1.15E-5 - 1.16E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.15E-5 - 1.16E-5 1/K

500.0 °C

1.19E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.19E-5 1/K

600.0 °C

1.21E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.21E-5 1/K

700.0 °C

1.24E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.24E-5 1/K

800.0 °C

1.29E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.29E-5 1/K

Unlock all property charts

Melting point

1370 - 1530 °C

Show Material materials with Melting point of 1370 - 1530 °C

Typical for Martensitic Stainless Steel

Specific heat capacity

20.0 °C

450 - 460 J/(kg·K)

Show Material materials with Specific heat capacity of 450 - 460 J/(kg·K)

100.0 °C

482 J/(kg·K)

Show Material materials with Specific heat capacity of 482 J/(kg·K)

200.0 °C

506 J/(kg·K)

Show Material materials with Specific heat capacity of 506 J/(kg·K)

300.0 °C

525 J/(kg·K)

Show Material materials with Specific heat capacity of 525 J/(kg·K)

400.0 °C

547 J/(kg·K)

Show Material materials with Specific heat capacity of 547 J/(kg·K)

500.0 °C

576 J/(kg·K)

Show Material materials with Specific heat capacity of 576 J/(kg·K)

600.0 °C

616 J/(kg·K)

Show Material materials with Specific heat capacity of 616 J/(kg·K)

Unlock all property charts

Thermal conductivity

20.0 °C

16 - 30 W/(m·K)

Show Material materials with Thermal conductivity of 16 - 30 W/(m·K)

100.0 °C

17.2 W/(m·K)

Show Material materials with Thermal conductivity of 17.2 W/(m·K)

200.0 °C

18.6 W/(m·K)

Show Material materials with Thermal conductivity of 18.6 W/(m·K)

300.0 °C

20 W/(m·K)

Show Material materials with Thermal conductivity of 20 W/(m·K)

400.0 °C

21.2 W/(m·K)

Show Material materials with Thermal conductivity of 21.2 W/(m·K)

500.0 °C

22.3 W/(m·K)

Show Material materials with Thermal conductivity of 22.3 W/(m·K)

600.0 °C

23.3 W/(m·K)

Show Material materials with Thermal conductivity of 23.3 W/(m·K)

700.0 °C

24.1 W/(m·K)

Show Material materials with Thermal conductivity of 24.1 W/(m·K)

800.0 °C

25.5 W/(m·K)

Show Material materials with Thermal conductivity of 25.5 W/(m·K)

900.0 °C

26.9 W/(m·K)

Show Material materials with Thermal conductivity of 26.9 W/(m·K)

1000.0 °C

28.3 W/(m·K)

Show Material materials with Thermal conductivity of 28.3 W/(m·K)

Unlock all property charts

Thermal diffusivity

20.0 °C

4.7 mm²/s

Show Material materials with Thermal diffusivity of 4.7 mm²/s

100.0 °C

4.5 mm²/s

Show Material materials with Thermal diffusivity of 4.5 mm²/s

200.0 °C

4.5 mm²/s

Show Material materials with Thermal diffusivity of 4.5 mm²/s

300.0 °C

4.6 mm²/s

Show Material materials with Thermal diffusivity of 4.6 mm²/s

400.0 °C

4.4 mm²/s

Show Material materials with Thermal diffusivity of 4.4 mm²/s

500.0 °C

4.1 mm²/s

Show Material materials with Thermal diffusivity of 4.1 mm²/s

600.0 °C

3.6 mm²/s

Show Material materials with Thermal diffusivity of 3.6 mm²/s

Unlock all property charts

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

6.5E-7 - 9.06E-7 Ω·m

Show Material materials with Electrical resistivity of 6.5E-7 - 9.06E-7 Ω·m

100.0 °C

9.42E-7 Ω·m

Show Material materials with Electrical resistivity of 9.42E-7 Ω·m

200.0 °C

9.87E-7 Ω·m

Show Material materials with Electrical resistivity of 9.87E-7 Ω·m

300.0 °C

1.03E-6 Ω·m

Show Material materials with Electrical resistivity of 1.03E-6 Ω·m

400.0 °C

1.08E-6 Ω·m

Show Material materials with Electrical resistivity of 1.08E-6 Ω·m

500.0 °C

1.12E-6 Ω·m

Show Material materials with Electrical resistivity of 1.12E-6 Ω·m

600.0 °C

1.18E-6 Ω·m

Show Material materials with Electrical resistivity of 1.18E-6 Ω·m

700.0 °C

1.22E-6 Ω·m

Show Material materials with Electrical resistivity of 1.22E-6 Ω·m

800.0 °C

1.24E-6 Ω·m

Show Material materials with Electrical resistivity of 1.24E-6 Ω·m

900.0 °C

1.26E-6 Ω·m

Show Material materials with Electrical resistivity of 1.26E-6 Ω·m

1000.0 °C

1.27E-6 Ω·m

Show Material materials with Electrical resistivity of 1.27E-6 Ω·m

Unlock all property charts

Chemical properties

PropertyValue

Carbon

0.45 - 0.55 %

Show Material materials with Carbon of 0.45 - 0.55 %

Chromium

14 - 15 %

Show Material materials with Chromium of 14 - 15 %

Manganese

1 %

Show Material materials with Manganese of 1 %

Molybdenum

0.5 - 0.8 %

Show Material materials with Molybdenum of 0.5 - 0.8 %

Phosphorus

0.04 %

Show Material materials with Phosphorus of 0.04 %

Silicon

1 %

Show Material materials with Silicon of 1 %

Sulfur

0.015 %

Show Material materials with Sulfur of 0.015 %

Vanadium

0.1 - 0.2 %